MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Overview of materials for Nylon 6, Impact Grade
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Impact Grade

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Nylon 6, Impact Grade". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.00 - 4.00 g/cc0.0361 - 0.145 lb/in³Average value: 1.15 g/cc Grade Count:418
 0.880 - 0.970 g/cc
@Temperature 220 - 325 °C
0.0318 - 0.0350 lb/in³
@Temperature 428 - 617 °F
Average value: 0.937 g/cc Grade Count:5
Filler Content 15.0 - 60.0 %15.0 - 60.0 %Average value: 37.1 % Grade Count:7
Water Absorption 0.0600 - 9.50 %0.0600 - 9.50 %Average value: 2.57 % Grade Count:201
Moisture Absorption at Equilibrium 0.170 - 8.00 %0.170 - 8.00 %Average value: 2.33 % Grade Count:122
 2.00 - 2.60 %
@Temperature 70.0 - 70.0 °C
2.00 - 2.60 %
@Temperature 158 - 158 °F
Average value: 2.30 % Grade Count:10
Water Absorption at Saturation 4.90 - 10.0 %4.90 - 10.0 %Average value: 7.81 % Grade Count:82
Viscosity  440000 - 440000 cP
@Temperature 280 - 280 °C
440000 - 440000 cP
@Temperature 536 - 536 °F
Average value: 440000 cP Grade Count:1
 440000 - 440000 cP
@Shear Rate 1000 - 1000 1/s
440000 - 440000 cP
@Shear Rate 1000 - 1000 1/s
Average value: 440000 cP Grade Count:1
Viscosity Test 125 - 150 cm³/g1.25 - 1.50 dl/gAverage value: 138 cm³/g Grade Count:11
Maximum Moisture Content 0.0200 - 0.2000.0200 - 0.200Average value: 0.100 Grade Count:10
 0.200 - 0.200
@Temperature 120 - 120 °C
0.200 - 0.200
@Temperature 248 - 248 °F
Average value: 0.200 Grade Count:1
 0.200 - 0.200
@Time 299 - 299 sec
0.200 - 0.200
@Time 0.0830 - 0.0830 hour
Average value: 0.200 Grade Count:1
Linear Mold Shrinkage 0.000100 - 0.0350 cm/cm0.000100 - 0.0350 in/inAverage value: 0.0118 cm/cm Grade Count:293
 0.0120 - 0.0130 cm/cm
@Temperature 80.0 - 80.0 °C
0.0120 - 0.0130 in/in
@Temperature 176 - 176 °F
Average value: 0.0125 cm/cm Grade Count:4
Linear Mold Shrinkage, Transverse 0.00100 - 0.0253 cm/cm0.00100 - 0.0253 in/inAverage value: 0.0130 cm/cm Grade Count:124
 0.0130 - 0.0150 cm/cm
@Temperature 80.0 - 80.0 °C
0.0130 - 0.0150 in/in
@Temperature 176 - 176 °F
Average value: 0.0140 cm/cm Grade Count:4
Melt Flow 3.00 - 121 g/10 min3.00 - 121 g/10 minAverage value: 33.9 g/10 min Grade Count:54
Spiral Flow 60.0 - 85.0 cm23.6 - 33.5 inAverage value: 68.3 cm Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 60.0 - 85.060.0 - 85.0Average value: 77.2 Grade Count:11
Hardness, Rockwell R 40.0 - 12540.0 - 125Average value: 106 Grade Count:96
 114 - 114
@Temperature 80.0 - 80.0 °C
114 - 114
@Temperature 176 - 176 °F
Average value: 114 Grade Count:1
Hardness, Shore D 47.0 - 82.047.0 - 82.0Average value: 66.6 Grade Count:19
Ball Indentation Hardness 30.0 - 220 MPa4350 - 31900 psiAverage value: 102 MPa Grade Count:37
Tensile Strength, Ultimate 12.0 - 470 MPa1740 - 68200 psiAverage value: 68.6 MPa Grade Count:192
 68.0 - 100 MPa
@Temperature -40.0 - -40.0 °C
9860 - 14500 psi
@Temperature -40.0 - -40.0 °F
Average value: 84.3 MPa Grade Count:7
Tensile Strength, Yield 25.0 - 207 MPa3630 - 30000 psiAverage value: 61.1 MPa Grade Count:238
 12.0 - 117 MPa
@Temperature -40.0 - 120 °C
1740 - 17000 psi
@Temperature -40.0 - 248 °F
Average value: 56.9 MPa Grade Count:8
Elongation at Break 1.50 - 500 %1.50 - 500 %Average value: 67.4 % Grade Count:368
 5.50 - 21.5 %
@Temperature -40.0 - 150 °C
5.50 - 21.5 %
@Temperature -40.0 - 302 °F
Average value: 33.2 % Grade Count:8
Elongation at Yield 2.10 - 350 %2.10 - 350 %Average value: 19.6 % Grade Count:123
 4.00 - 37.0 %
@Temperature -40.0 - 120 °C
4.00 - 37.0 %
@Temperature -40.0 - 248 °F
Average value: 23.7 % Grade Count:6
Modulus of Elasticity 0.150 - 1090 GPa21.8 - 158000 ksiAverage value: 7.04 GPa Grade Count:217
 0.145 - 3.30 GPa
@Temperature -40.0 - 150 °C
21.0 - 479 ksi
@Temperature -40.0 - 302 °F
Average value: 0.997 GPa Grade Count:8
Flexural Yield Strength 9.65 - 310 MPa1400 - 45000 psiAverage value: 91.9 MPa Grade Count:277
 8.00 - 148 MPa
@Temperature -40.0 - 120 °C
1160 - 21500 psi
@Temperature -40.0 - 248 °F
Average value: 64.2 MPa Grade Count:11
Flexural Modulus 0.0689 - 14.0 GPa10.0 - 2030 ksiAverage value: 2.61 GPa Grade Count:330
 0.145 - 2.60 GPa
@Temperature -40.0 - 120 °C
21.0 - 377 ksi
@Temperature -40.0 - 248 °F
Average value: 0.892 GPa Grade Count:8
Flexural Strain at Break 3.70 - 9.00 %3.70 - 9.00 %Average value: 6.01 % Grade Count:15
Compressive Yield Strength 24.0 - 125 MPa3480 - 18100 psiAverage value: 61.6 MPa Grade Count:7
Poissons Ratio 0.350 - 0.4700.350 - 0.470Average value: 0.407 Grade Count:13
Izod Impact, Notched 0.0850 J/cm - NB0.159 ft-lb/in - NBAverage value: 4.69 J/cm Grade Count:175
 0.350 - 7.30 J/cm
@Temperature -40.0 - -20.0 °C
0.656 - 13.7 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 1.67 J/cm Grade Count:14
 0.588399 - 5338.47 J/cm
@Temperature -40.0 - -20.0 °C
1.10231 - 10001.1 ft-lb/in
@Temperature -40.0 - -4.00 °F
Average value: 1.67 J/cm Grade Count:22
 0.588399 - 5338.47 J/cm
@Thickness 3.17 - 6.40 mm
1.10231 - 10001.1 ft-lb/in
@Thickness 0.125 - 0.252 in
Average value: 1.67 J/cm Grade Count:22
Izod Impact, Unnotched 13.9 J/cm - NB26.0 ft-lb/in - NBAverage value: 14.6 J/cm Grade Count:35
Izod Impact, Notched (ISO) 4.00 kJ/m² - NB1.90 ft-lb/in² - NBAverage value: 34.5 kJ/m² Grade Count:99
 5.00 - 85.0 kJ/m²
@Temperature -40.0 - -30.0 °C
2.38 - 40.4 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 16.8 kJ/m² Grade Count:42
Izod Impact, Unnotched (ISO) 50.0 kJ/m² - NB23.8 ft-lb/in² - NBAverage value: 77.0 kJ/m² Grade Count:27
 40.0 kJ/m² - NB
@Temperature -30.0 - -30.0 °C
19.0 ft-lb/in² - NB
@Temperature -22.0 - -22.0 °F
Average value: 69.5 kJ/m² Grade Count:21
Charpy Impact Unnotched 0.450 J/cm² - NB2.14 ft-lb/in² - NBAverage value: 11.3 J/cm² Grade Count:175
 4.00 J/cm² - NB
@Temperature -70.0 - -20.0 °C
19.0 ft-lb/in² - NB
@Temperature -94.0 - -4.00 °F
Average value: 8.36 J/cm² Grade Count:110
Charpy Impact, Notched 0.400 J/cm² - NB1.90 ft-lb/in² - NBAverage value: 4.21 J/cm² Grade Count:215
 0.300 - 2099.79 J/cm²
@Temperature -40.0 - -20.0 °C
1.43 - 9993.41 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 1.74 J/cm² Grade Count:114
Gardner Impact 36.2 J26.7 ft-lbAverage value: 36.2 J Grade Count:4
Dart Drop, Total Energy 45.0 - 45.0 J
@Temperature -20.0 - -20.0 °C
33.2 - 33.2 ft-lb
@Temperature -4.00 - -4.00 °F
Average value: 45.0 J Grade Count:1
Puncture Energy 16.0 - 64.0 J11.8 - 47.2 ft-lbAverage value: 48.0 J Grade Count:3
 25.0 - 64.0 J
@Temperature -30.0 - -30.0 °C
18.4 - 47.2 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 54.3 J Grade Count:2
 64.0 - 64.0 J
@Temperature -30.0 - -30.0 °C
47.2 - 47.2 ft-lb
@Temperature -22.0 - -22.0 °F
Average value: 54.3 J Grade Count:1
 64.0 - 64.0 J
@Load <=5810 kg
47.2 - 47.2 ft-lb
@Load <=12800 lb
Average value: 54.3 J Grade Count:1
Taber Abrasion, mg/1000 Cycles 6.00 - 19.06.00 - 19.0Average value: 10.8 Grade Count:7
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 100 - 1.00e+16 ohm-cm100 - 1.00e+16 ohm-cmAverage value: 5.47e+14 ohm-cm Grade Count:187
Surface Resistance 100 - 1.00e+15 ohm100 - 1.00e+15 ohmAverage value: 1.05e+14 ohm Grade Count:103
Dielectric Constant 2.70 - 15.42.70 - 15.4Average value: 5.45 Grade Count:82
Dielectric Strength 11.8 - 100 kV/mm300 - 2540 kV/inAverage value: 28.1 kV/mm Grade Count:150
Dissipation Factor 0.00300 - 0.4000.00300 - 0.400Average value: 0.102 Grade Count:37
Dielectric Loss Index 0.0190 - 0.3000.0190 - 0.300Average value: 0.132 Grade Count:13
Arc Resistance 113 - 195 sec113 - 195 secAverage value: 156 sec Grade Count:13
Comparative Tracking Index 400 - 600 V400 - 600 VAverage value: 570 V Grade Count:98
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.00 - 200 µm/m-°C3.89 - 111 µin/in-°FAverage value: 76.2 µm/m-°C Grade Count:138
 91.0 - 91.0 µm/m-°C
@Temperature 55.0 - 160 °C
50.6 - 50.6 µin/in-°F
@Temperature 131 - 320 °F
Average value: 91.0 µm/m-°C Grade Count:1
CTE, linear, Transverse to Flow 50.0 - 190 µm/m-°C27.8 - 106 µin/in-°FAverage value: 118 µm/m-°C Grade Count:46
 86.0 - 86.0 µm/m-°C
@Temperature 55.0 - 160 °C
47.8 - 47.8 µin/in-°F
@Temperature 131 - 320 °F
Average value: 86.0 µm/m-°C Grade Count:1
Specific Heat Capacity 1.50 - 3.89 J/g-°C0.359 - 0.930 BTU/lb-°FAverage value: 2.50 J/g-°C Grade Count:5
 2.22 - 2.60 J/g-°C
@Temperature 270 - 325 °C
0.531 - 0.621 BTU/lb-°F
@Temperature 518 - 617 °F
Average value: 2.47 J/g-°C Grade Count:3
Thermal Conductivity 0.168 - 0.320 W/m-K1.17 - 2.22 BTU-in/hr-ft²-°FAverage value: 0.249 W/m-K Grade Count:7
 0.150 - 0.180 W/m-K
@Temperature 270 - 325 °C
1.04 - 1.25 BTU-in/hr-ft²-°F
@Temperature 518 - 617 °F
Average value: 0.160 W/m-K Grade Count:3
Melting Point 205 - 300 °C401 - 572 °FAverage value: 221 °C Grade Count:225
Maximum Service Temperature, Air 55.0 - 200 °C131 - 392 °FAverage value: 124 °C Grade Count:33
Hot Ball Pressure Test 125 - 165 °C257 - 329 °FAverage value: 138 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 50.0 - 221 °C122 - 430 °FAverage value: 155 °C Grade Count:191
Deflection Temperature at 1.8 MPa (264 psi) 35.0 - 213 °C95.0 - 415 °FAverage value: 83.9 °C Grade Count:304
Deflection Temperature at 8.0 MPa 40.0 - 125 °C104 - 257 °FAverage value: 73.5 °C Grade Count:8
Vicat Softening Point 95.0 - 225 °C203 - 437 °FAverage value: 185 °C Grade Count:63
Minimum Service Temperature, Air -100 - -40.0 °C-148 - -40.0 °FAverage value: -60.0 °C Grade Count:5
Glass Transition Temp, Tg 0.000 - 60.0 °C32.0 - 140 °FAverage value: 35.8 °C Grade Count:7
UL RTI, Electrical 60.0 - 65.0 °C140 - 149 °FAverage value: 61.7 °C Grade Count:3
UL RTI, Mechanical with Impact 60.0 - 65.0 °C140 - 149 °FAverage value: 61.7 °C Grade Count:3
UL RTI, Mechanical without Impact 60.0 - 65.0 °C140 - 149 °FAverage value: 61.7 °C Grade Count:3
Flammability, UL94 HB - V-0HB - V-0Grade Count:193
Flame Spread 10.0 - 100 mm/min0.394 - 3.94 in/minAverage value: 69.0 mm/min Grade Count:10
Oxygen Index 21.0 - 23.0 %21.0 - 23.0 %Average value: 21.9 % Grade Count:8
Glow Wire Test 650 - 850 °C1200 - 1560 °FAverage value: 709 °C Grade Count:26
 
Processing PropertiesMetricEnglishComments
Processing Temperature 221 - 300 °C430 - 572 °FAverage value: 260 °C Grade Count:34
Nozzle Temperature 230 - 299 °C446 - 570 °FAverage value: 260 °C Grade Count:30
Melt Temperature 210 - 330 °C410 - 626 °FAverage value: 257 °C Grade Count:154
Mold Temperature 21.1 - 120 °C70.0 - 248 °FAverage value: 71.3 °C Grade Count:175
Drying Temperature 60.0 - 120 °C140 - 248 °FAverage value: 82.2 °C Grade Count:132
Moisture Content 0.000 - 0.200 %0.000 - 0.200 %Average value: 0.158 % Grade Count:67
Dew Point -40.0 - -17.8 °C-40.0 - 0.000 °FAverage value: -28.9 °C Grade Count:4
Injection Pressure 4.14 - 150 MPa600 - 21800 psiAverage value: 67.9 MPa Grade Count:35

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Nylon 6, Unreinforced
Overview of materials for Nylon 6, Cast
Overview of materials for Nylon 6, 20% Glass Fiber Filled
Overview of materials for Nylon 66, Impact Grade
Overview of materials for Nylon 6, 10% Glass Fiber Filled

O2401 / 77962

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.