MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Telles Mirel™ P2001 Bioplastic, Extrusion Coating Grade  (discontinued **)
Categories: Polymer; Renewable/Recycled Polymer; Thermoplastic; Polyester, TP

Material Notes: Mirel™ P2001 is a high performance, semi-crystalline natural polyester specifically engineered for extrusion coating of paperboard. Mirel resins are innovative and versatile solutions suitable for a wide variety of product applications.

Environmental Innovation: Environmental responsibility is a major trend among industry leading brand owners and OEMs. Mirel is a new family of biobased resin providing the industry with sustainable alternatives to conventional plastics. Mirel meets the demands of environmentally-conscious companies and consumers making a positive impact on global climate change. Mirel starts with nature and ends with nature. It harmlessly biodegrades in all of these environments:

  • Industrial and home composting
  • Soil
  • Municipal waste treatment facilities, septic systems
  • Wetlands, streams, and oceans.

Potential Applications:

  • Food service ware-Cups and containers; Food cartons; Single serve disposables
  • Food storage - Freezer cartons; Beverage or food storage boxes
Product Attributes
  • Heat sealable
  • Good printability
  • Good barrier properties
  • Adhesion to substrates
Biodegradation Certifications and Testing: Mirel resins are certified to ASTM D6400 / EN 13432 for compostable plastics, and D7081 / EN 17556 for non-floating biodegradable plastics in marine environment. Test results from ASTM D5988-96 / ISO 17556 for aerobic biodegradation in soil of plastics or residual plastics materials show that Mirel fully biodegrades - fungal/bacterial under ambient conditions. Test results from ASTM D5209 / ISO 14852 / ASTM D5271 / 14851 for aerobic biodegradation of plastic materials in an activated-sludge wastewater-treatment system show that fully biodegrades - bacterial under ambient conditions.

Property data listed measured after 21 day aging.

Telles is a joint venture between Metabolix and Archer Daniels Midland Company.

Key Words: Polyhydroxyalkanoate
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.24 g/cc1.24 g/ccASTM D792
Water Absorption 0.10 %0.10 %24 hrs; ASTM D570
Viscosity 0.75 cP
@Shear Rate 100 1/s,
Temperature 180 °C
0.75 cP
@Shear Rate 100 1/s,
Temperature 356 °F
ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 28.0 MPa4060 psiISO 527-1, -2
 29.6 MPa4300 psiASTM D638
Elongation at Break 7.0 %7.0 %ISO 527-1, -2
 7.0 %7.0 %ASTM D638
Flexural Strength 36.0 MPa5220 psiISO 178
 42.7 MPa6200 psiASTM D790 A
Flexural Modulus 1.59 GPa230 ksiASTM D790 A
 1.70 GPa247 ksiISO 178
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 123 °C253 °FISO 75-1 B
 132 °C270 °FASTM D648 B
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °C144 °FISO 75-1 A
 63.9 °C147 °FASTM D648 B
Vicat Softening Point 137 °C278 °FASTM D1525 A10
 137 °C279 °FISO 306 A50
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 175 - 180 °C347 - 356 °F
Middle Barrel Temperature 175 - 180 °C347 - 356 °F
Front Barrel Temperature 170 - 175 °C338 - 347 °FNote reverse temperature profile
Adapter Temperature 165 - 170 °C329 - 338 °FDraw ratio < 10:1
Melt Temperature 160 - 175 °C320 - 347 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2 - 4 hour2 - 4 hour

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Telles Mirel™ P1003 Injection Molding Grade PHA Bioplastic
NatureWorks® Ingeo™ AW 240D Biopolymer for Food Serviceware
NatureWorks® Ingeo™ AW 300D Injection Grade Biopolymer
Telles Mirel™ P5001 Film Grade PHA Bioplastic
LyondellBasell Hostacom™ RE-44AC Thermoplastic Polyolefin Elastomer

PMETAA993 / 78810

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.