MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

AISI Type 420F Stainless Steel, annealed and cold drawn wire
Categories: Metal; Ferrous Metal; Heat Resisting; Stainless Steel; T 400 Series Stainless Steel

Material Notes:

Key Words: UNS S42020, AMS 5620, SAE J405 (51420F), martensitic
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 9999
Tensile Strength, Ultimate 690 MPa100000 psi
Tensile Strength, Yield 550 MPa
@Strain 0.2 %
79800 psi
@Strain 0.2 %
Elongation at Break 15 %15 %in 50 mm
Modulus of Elasticity 200 GPa29000 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000550 ohm-cm
@Temperature 20.0 °C
0.0000550 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.3 µm/m-°C
@Temperature 0.000 - 100 °C
5.72 µin/in-°F
@Temperature 32.0 - 212 °F
 12.2 µm/m-°C
@Temperature 0.000 - 650 °C
6.78 µin/in-°F
@Temperature 32.0 - 1200 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 0.000 - 100 °C
0.110 BTU/lb-°F
@Temperature 32.0 - 212 °F
Thermal Conductivity 25.1 W/m-K
@Temperature 27.0 °C
174 BTU-in/hr-ft²-°F
@Temperature 80.6 °F
Melting Point 1455 - 1510 °C2651 - 2750 °F
Solidus 1455 °C2651 °F
Liquidus 1510 °C2750 °F
Maximum Service Temperature, Air 620 °C1150 °FContinuous Service
 735 °C1360 °FIntermittent
 
Component Elements PropertiesMetricEnglishComments
Carbon, C >= 0.15 %>= 0.15 %
Chromium, Cr 13 %13 %
Iron, Fe 84 %84 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo <= 0.60 %<= 0.60 %Optional
Phosphorus, P <= 0.040 %<= 0.040 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S >= 0.15 %>= 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
416 Stainless Steel, annealed wire 6.4 mm diameter
416 Stainless Steel, annealed bar
422 Stainless Steel, 455°C temper, short time elevated temperature test
AISI Type 420F Stainless Steel, annealed and cold drawn bar
AISI Type 420F Stainless Steel, annealed bar

MQ420S / 13080

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.