MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 25 alloy, cold rolled and 1205°C (2200°F) solution annealed sheet
Categories: Metal; Nonferrous Metal; Cobalt Alloy; Superalloy

Material Notes: Excellent high-temperature strength with good resistance to oxidizing environments up to 980°C for prolonged exposures and excellent resistance to sulfidation and excellent resistance to metal galling. Applications in the aerospace industry, including parts in military and commercial gas turbine engines.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS R30605, AMS 5537, AMS 5759, AMS 5796, AMS 5795
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 9.13 g/cc0.330 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 1005 MPa145800 psi
 160 MPa
@Temperature 1095 °C
23200 psi
@Temperature 2003 °F
 235 MPa
@Temperature 980 °C
34100 psi
@Temperature 1800 °F
 415 MPa
@Temperature 870 °C
60200 psi
@Temperature 1600 °F
 640 MPa
@Temperature 760 °C
92800 psi
@Temperature 1400 °F
 745 MPa
@Temperature 650 °C
108000 psi
@Temperature 1200 °F
 770 MPa
@Temperature 540 °C
112000 psi
@Temperature 1000 °F
Tensile Strength, Yield 475 MPa
@Strain 0.2 %
68900 psi
@Strain 0.2 %
 76.0 MPa
@Strain 0.2 %,
Temperature 1095 °C
11000 psi
@Strain 0.2 %,
Temperature 2003 °F
 125 MPa
@Strain 0.2 %,
Temperature 980 °C
18100 psi
@Strain 0.2 %,
Temperature 1800 °F
 250 MPa
@Strain 0.2 %,
Temperature 870 °C
36300 psi
@Strain 0.2 %,
Temperature 1600 °F
 285 MPa
@Strain 0.2 %,
Temperature 760 °C
41300 psi
@Strain 0.2 %,
Temperature 1400 °F
 330 MPa
@Strain 0.2 %,
Temperature 540 °C
47900 psi
@Strain 0.2 %,
Temperature 1000 °F
 330 MPa
@Strain 0.2 %,
Temperature 650 °C
47900 psi
@Strain 0.2 %,
Temperature 1200 °F
Elongation at Break 51 %51 %in 51 mm
 36 %
@Temperature 980 °C
36 %
@Temperature 1800 °F
in 51 mm
 42 %
@Temperature 760 °C
42 %
@Temperature 1400 °F
in 51 mm
 45 %
@Temperature 870 °C
45 %
@Temperature 1600 °F
in 51 mm
 48 %
@Temperature 1095 °C
48 %
@Temperature 2003 °F
in 51 mm
 60 %
@Temperature 540 °C
60 %
@Temperature 1000 °F
in 51 mm
 60 %
@Temperature 650 °C
60 %
@Temperature 1200 °F
in 51 mm
Modulus of Elasticity 225 GPa32600 ksiRT
 146 GPa
@Temperature 1000 °C
21200 ksi
@Temperature 1830 °F
 154 GPa
@Temperature 900 °C
22300 ksi
@Temperature 1650 °F
 163 GPa
@Temperature 800 °C
23600 ksi
@Temperature 1470 °F
 174 GPa
@Temperature 700 °C
25200 ksi
@Temperature 1290 °F
 181 GPa
@Temperature 600 °C
26300 ksi
@Temperature 1110 °F
 188 GPa
@Temperature 500 °C
27300 ksi
@Temperature 932 °F
 197 GPa
@Temperature 400 °C
28600 ksi
@Temperature 752 °F
 204 GPa
@Temperature 300 °C
29600 ksi
@Temperature 572 °F
 214 GPa
@Temperature 200 °C
31000 ksi
@Temperature 392 °F
 222 GPa
@Temperature 100 °C
32200 ksi
@Temperature 212 °F
Charpy Impact 262 J193 ft-lb
 144 J
@Temperature 980 °C
106 ft-lb
@Temperature 1800 °F
 148 J
@Temperature -196 °C
109 ft-lb
@Temperature -321 °F
 163 J
@Temperature 870 °C
120 ft-lb
@Temperature 1600 °F
 182 J
@Temperature -138 °C
134 ft-lb
@Temperature -216 °F
 194 J
@Temperature 760 °C
143 ft-lb
@Temperature 1400 °F
 212 J
@Temperature -78.0 °C
156 ft-lb
@Temperature -108 °F
 230 J
@Temperature 650 °C
170 ft-lb
@Temperature 1200 °F
 243 J
@Temperature -29.0 °C
179 ft-lb
@Temperature -20.2 °F
 273 J
@Temperature 540 °C
201 ft-lb
@Temperature 1000 °F
 297 J
@Temperature 260 °C
219 ft-lb
@Temperature 500 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000886 ohm-cm0.0000886 ohm-cmRT
 0.0000950 ohm-cm
@Temperature 1000 °C
0.0000950 ohm-cm
@Temperature 1830 °F
 0.0001011 ohm-cm
@Temperature 900 °C
0.0001011 ohm-cm
@Temperature 1650 °F
 0.0001066 ohm-cm
@Temperature 700 °C
0.0001066 ohm-cm
@Temperature 1290 °F
 0.0001078 ohm-cm
@Temperature 800 °C
0.0001078 ohm-cm
@Temperature 1470 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.3 µm/m-°C
@Temperature 25.0 - 100 °C
6.83 µin/in-°F
@Temperature 77.0 - 212 °F
 12.9 µm/m-°C
@Temperature 25.0 - 200 °C
7.17 µin/in-°F
@Temperature 77.0 - 392 °F
 13.6 µm/m-°C
@Temperature 25.0 - 300 °C
7.56 µin/in-°F
@Temperature 77.0 - 572 °F
 14.3 µm/m-°C
@Temperature 25.0 - 500 °C
7.94 µin/in-°F
@Temperature 77.0 - 932 °F
 14.3 µm/m-°C
@Temperature 25.0 - 400 °C
7.94 µin/in-°F
@Temperature 77.0 - 752 °F
 14.6 µm/m-°C
@Temperature 25.0 - 600 °C
8.11 µin/in-°F
@Temperature 77.0 - 1110 °F
 15.1 µm/m-°C
@Temperature 25.0 - 700 °C
8.39 µin/in-°F
@Temperature 77.0 - 1290 °F
 15.8 µm/m-°C
@Temperature 25.0 - 800 °C
8.78 µin/in-°F
@Temperature 77.0 - 1470 °F
 16.5 µm/m-°C
@Temperature 25.0 - 900 °C
9.17 µin/in-°F
@Temperature 77.0 - 1650 °F
 17.0 µm/m-°C
@Temperature 25.0 - 1000 °C
9.44 µin/in-°F
@Temperature 77.0 - 1830 °F
Thermal Conductivity 9.40 W/m-K65.2 BTU-in/hr-ft²-°FRT
 10.9 W/m-K
@Temperature 100 °C
75.6 BTU-in/hr-ft²-°F
@Temperature 212 °F
 12.9 W/m-K
@Temperature 200 °C
89.5 BTU-in/hr-ft²-°F
@Temperature 392 °F
 14.8 W/m-K
@Temperature 300 °C
103 BTU-in/hr-ft²-°F
@Temperature 572 °F
 16.8 W/m-K
@Temperature 400 °C
117 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.7 W/m-K
@Temperature 500 °C
130 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.7 W/m-K
@Temperature 600 °C
144 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.6 W/m-K
@Temperature 700 °C
157 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.7 W/m-K
@Temperature 800 °C
171 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 26.7 W/m-K
@Temperature 900 °C
185 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 29.2 W/m-K
@Temperature 1000 °C
203 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1330 - 1410 °C2430 - 2570 °F
Solidus 1330 °C2430 °F
Liquidus 1410 °C2570 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.10 %0.10 %
Chromium, Cr 20 %20 %
Cobalt, Co 51 %51 %
Iron, Fe <= 3.0 %<= 3.0 %
Manganese, Mn 1.5 %1.5 %
Nickel, Ni 10 %10 %
Silicon, Si <= 0.40 %<= 0.40 %
Tungsten, W 15 %15 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Universal Wire Works Haynes 25 (L-605) (AMS 5796) Filler Metal
ATI Allvac® Nickelvac® L-605 Cobalt-Nickel Superalloy, Heat Treatment: 1204°C (2200°F) Anneal
Haynes 25 alloy, cold worked sheet, 10% cold reduction
ATI Allvac® 35N Nickel Superalloy BIllet, Heat Treatment: 1052°C (1925°F) + Age
Carpenter MP35N* Ni-Co-Cr-Mo Alloy, 0% Cold Reduction

NH25AA / 16554

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.