MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

NOVA Chemicals Novapol® HE-Y449-AC HDPE Extrusion Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Extruded

Material Notes: Medium molecular weight HDPE, Good toughness, Good chemical resistance, Good processability

Applications: Corrugated tubing, Conduit

Additives: Antioxidants

Information provided by NOVA Chemicals.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.946 g/cc0.0342 lb/in³ASTM D792
ESCR 100% Igepal® >= 1000 hour
@Temperature 50.0 °C
>= 1000 hour
@Temperature 122 °F
F50; Condition B; ASTM D1693
Oxidative Induction Time (OIT) 10 min10 minCondition 220°C in oxygen gas environment; ASTM D3895
Melt Flow 0.40 g/10 min
@Load 2.16 kg,
Temperature 190 °C
0.40 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6161ASTM D2240
Tensile Strength, Yield 24.0 MPa3480 psiExtension rate 2 in/min; ASTM D638
Elongation at Break 650 %650 %Extension rate 2 in/min; ASTM D638
Flexural Modulus 1.14 GPa165 ksiTangent; ASTM D790
Izod Impact, Notched 0.800 J/cm1.50 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Melting Point 130 °C266 °FASTM D3417
Vicat Softening Point 124 °C255 °FASTM D1525
Brittleness Temperature <= -100 °C<= -148 °FASTM D746

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
NOVA Chemicals Sclair® SD-7250-0B HDPE Extrusion Resin
JPJ Technologies 7800M HDPE Extrusion
Overview of materials for High Density Polyethylene (HDPE), Extruded
Ineos K44-06-123 Extrusion Grade Polyethylene
Baystar™ 7195 High Density Polyethylene, Specialty Extrusion Resin

PNOVA121 / 55022

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.