MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Latrobe TNW™ ASTM M10 High Speed Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Carbon Steel; High Carbon Steel; Tool Steel

Material Notes: TNW is an M10 type high speed steel with a composition that combines the high toughness of a high-molybdenum steel and the excellent wear resistance provided by the 2% vanadium content. TNW is popular for twist drills, reamers, taps, router bits, end mills and similar cutting tools. Its good toughness makes it well suited for punches and other cold work tools that require high hardness and wear resistance.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 7.89 g/cc7.89 g/cc
Density 7.89 g/cc0.285 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C  40
@Temperature 650 °C
40
@Temperature 1200 °F
Oil Quenched from 1218°C; 566°C Double Temper Temperature
 60.5
@Temperature 316 °C
60.5
@Temperature 601 °F
Oil Quenched from 1218°C; 566°C Double Temper Temperature
 65
@Temperature 22.0 °C
65
@Temperature 71.6 °F
Oil Quenched from 1218°C; 566°C Double Temper Temperature
Modulus of Elasticity 207 GPa30000 ksi
Machinability 50 - 55 %50 - 55 %1% Carbon Steel
Izod Impact Unnotched 47.5 J35.0 ft-lbOil Quenched at 1218°C; 482°C Temper Temperature
 58.3 J43.0 ft-lbOil Quenched at 1218°C; 566°C Temper Temperature
 59.7 J44.0 ft-lbOil Quenched at 1218°C; 622°C Temper Temperature
 73.2 J54.0 ft-lbOil Quenched at 1163°C; 482°C
 88.1 J65.0 ft-lbOil Quenched at 1163°C; 622°C
 107 J79.0 ft-lbOil Quenched at 1163°C; 594°C
 
Thermal PropertiesMetricEnglishComments
CTE, linear  10.79 µm/m-°C
@Temperature 38.0 - 260 °C
5.994 µin/in-°F
@Temperature 100 - 500 °F
 12.58 µm/m-°C
@Temperature 38.0 - 649 °C
6.989 µin/in-°F
@Temperature 100 - 1200 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 774 °C1430 °FCritical Temperaure Ar3
 804 °C1480 °FCritical Temperaure Ar1
 830 °C1530 °FCritical Temperaure Ac1
 857 °C1570 °FCritical Temperaure Ac3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.87 %0.87 %
Chromium, Cr 4.0 %4.0 %
Iron, Fe 84.63 %84.63 %
Manganese, Mn 0.30 %0.30 %
Molybdenum, Mo 8.0 %8.0 %
Silicon, Si 0.30 %0.30 %
Vanadium, V 1.9 %1.9 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Latrobe Tatmo™ ASTM M1 High Speed Steel
AISI 1005 Steel
ASTM A485 Steel, Grade 2
ASTM A514 Steel, grade P, plate thickness ≤ 19 mm
ASTM A570 Steel, grade 33

NTIMK069 / 19416

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.