MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Latrobe TNW™ ASTM M10 High Speed Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Carbon Steel; High Carbon Steel; Tool Steel

Material Notes: TNW is an M10 type high speed steel with a composition that combines the high toughness of a high-molybdenum steel and the excellent wear resistance provided by the 2% vanadium content. TNW is popular for twist drills, reamers, taps, router bits, end mills and similar cutting tools. Its good toughness makes it well suited for punches and other cold work tools that require high hardness and wear resistance.

Information Provided by Timken Latrobe Steel.

Timken sold Latrobe in December 2006. They are now Latrobe Specialty Steels Co.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 7.89 g/cc
Density 0.285 lb/in³
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell C 40
@Temperature 650 °C
Oil Quenched from 1218°C; 566°C Double Temper Temperature
 60.5
@Temperature 316 °C
Oil Quenched from 1218°C; 566°C Double Temper Temperature
 65
@Temperature 22.0 °C
Oil Quenched from 1218°C; 566°C Double Temper Temperature
Modulus of Elasticity 30000 ksi
Machinability 50 - 55 %1% Carbon Steel
Izod Impact Unnotched 35.0 ft-lbOil Quenched at 1218°C; 482°C Temper Temperature
 43.0 ft-lbOil Quenched at 1218°C; 566°C Temper Temperature
 44.0 ft-lbOil Quenched at 1218°C; 622°C Temper Temperature
 54.0 ft-lbOil Quenched at 1163°C; 482°C
 65.0 ft-lbOil Quenched at 1163°C; 622°C
 79.0 ft-lbOil Quenched at 1163°C; 594°C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.79 µm/m-°C
@Temperature 38.0 - 260 °C
 12.58 µm/m-°C
@Temperature 38.0 - 649 °C
 
Processing PropertiesOriginal ValueComments
Processing Temperature 774 °CCritical Temperaure Ar3
 804 °CCritical Temperaure Ar1
 830 °CCritical Temperaure Ac1
 857 °CCritical Temperaure Ac3
 
Component Elements PropertiesOriginal ValueComments
Carbon, C 0.87 %
Chromium, Cr 4.0 %
Iron, Fe 84.63 %
Manganese, Mn 0.30 %
Molybdenum, Mo 8.0 %
Silicon, Si 0.30 %
Vanadium, V 1.9 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Latrobe Tatmo™ ASTM M1 High Speed Steel
AISI 1005 Steel
ASTM A485 Steel, Grade 2
ASTM A514 Steel, grade P, plate thickness ≤ 19 mm
ASTM A570 Steel, grade 33

NTIMK069 / 19416

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.