Physical Properties | Original Value | Comments |
---|
Density | 1.03 g/cc |
Water Absorption | 1.30 % |
Moisture Absorption | 0.500 % |
Linear Mold Shrinkage, Flow | 0.00700 cm/cm |
Linear Mold Shrinkage, Transverse | 0.0130 cm/cm |
Melt Flow | 9.00 g/10 min @Load 5.00 kg, Temperature 230 °C |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength at Break | 42.0 MPa |
Tensile Strength | 28.0 MPa |
Tensile Stress | 28.0 MPa @Strain 50.0 % |
| 9.00 MPa @Strain 10.0 %, Temperature 120 °C |
| 10.0 MPa @Strain 10.0 %, Temperature 100 °C |
| 10.0 MPa @Strain 50.0 %, Temperature 120 °C |
| 13.0 MPa @Strain 10.0 %, Temperature 80.0 °C |
| 15.0 MPa @Strain 10.0 %, Temperature 60.0 °C |
| 15.0 MPa @Strain 50.0 %, Temperature 100 °C |
| 17.0 MPa @Strain 50.0 %, Temperature 80.0 °C |
| 20.0 MPa @Strain 9.00 %, Temperature 23.0 °C |
| 20.0 MPa @Strain 15.0 %, Temperature 40.0 °C |
| 20.0 MPa @Strain 50.0 %, Temperature 60.0 °C |
| 20.0 MPa @Strain 1.00 %, Temperature -40.0 °C |
| 20.0 MPa @Strain 2.00 %, Temperature -20.0 °C |
| 20.0 MPa @Strain 4.00 %, Temperature 0.000 °C |
| 23.0 MPa @Strain 50.0 %, Temperature 40.0 °C |
| 25.0 MPa @Strain 50.0 %, Temperature 23.0 °C |
| 35.0 MPa @Strain 25.0 %, Temperature 0.000 °C |
| 50.0 MPa @Strain 20.0 %, Temperature -20.0 °C |
| 65.0 MPa @Strain 10.0 %, Temperature -40.0 °C |
Tensile Strength, Yield | 28.0 MPa |
Elongation at Break | 210 % |
Elongation at Yield | 33.0 % |
Tensile Modulus | 400 MPa |
Flexural Modulus | 400 MPa |
Secant Modulus | 0.0400 GPa @Strain 50.0 %, Temperature 120 °C |
| 0.0500 GPa @Strain 50.0 %, Temperature 100 °C |
| 0.0600 GPa @Strain 50.0 %, Temperature 80.0 °C |
| 0.0700 GPa @Strain 50.0 %, Temperature 60.0 °C |
| 0.0800 GPa @Strain 50.0 %, Temperature 40.0 °C |
| 0.0900 GPa @Strain 50.0 %, Temperature 23.0 °C |
| 0.100 GPa @Strain 2.00 %, Temperature 120 °C |
| 0.150 GPa @Strain 2.00 %, Temperature 100 °C |
| 0.200 GPa @Strain 2.00 %, Temperature 80.0 °C |
| 0.200 GPa @Strain 25.0 %, Temperature 0.000 °C |
| 0.250 GPa @Strain 2.00 %, Temperature 60.0 °C |
| 0.300 GPa @Strain 2.00 %, Temperature 40.0 °C |
| 0.300 GPa @Strain 20.0 %, Temperature -20.0 °C |
| 0.350 GPa @Strain 2.00 %, Temperature 23.0 °C |
| 0.750 GPa @Strain 10.0 %, Temperature -40.0 °C |
| 0.750 GPa @Strain 1.00 %, Temperature 0.000 °C |
| 1.25 GPa @Strain 1.00 %, Temperature -20.0 °C |
| 2.40 GPa @Strain 0.000 %, Temperature -40.0 °C |
Charpy Impact Unnotched | NB @Temperature 23.0 °C |
| NB @Temperature -30.0 °C |
Charpy Impact, Notched | 6.00 kJ/m² @Temperature -30.0 °C |
| 150 kJ/m² @Temperature 23.0 °C |
|
Electrical Properties | Original Value | Comments |
---|
Volume Resistivity | 1.00e+10 ohm-cm |
Dielectric Constant | 3.80 @Frequency 1.00e+6 Hz |
| 12.0 @Frequency 100 Hz |
Dielectric Strength | 32.0 kV/mm |
| 37.0 kV/mm |
Dissipation Factor | 0.150 @Frequency 1.00e+6 Hz |
| 0.160 @Frequency 100 Hz |
Comparative Tracking Index | 600 V |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear, Parallel to Flow | 170 µm/m-°C @Temperature 25.0 - 55.0 °C |
CTE, linear, Transverse to Flow | 160 µm/m-°C @Temperature 25.0 - 55.0 °C |
Melting Point | 171 °C |
Deflection Temperature at 0.46 MPa (66 psi) | 98.0 °C |
Deflection Temperature at 1.8 MPa (264 psi) | 45.0 °C |
Vicat Softening Point | 125 °C @Load 5.10 kg |
| 165 °C @Load 1.02 kg |
Flammability, UL94 | HB @Thickness 1.30 mm |
| HB @Thickness 3.20 mm |
|
Processing Properties | Original Value | Comments |
---|
Melt Temperature | 220 °C |
| 220 °C |
Mold Temperature | 60.0 °C |
| 60.0 °C |
Injection Velocity | 200 mm/sec |
Injection Pressure | 70.0 MPa |
|
Descriptive Properties |
---|
Blue water consumption | 25.9 kg |
Color | Black |
Global Warming Potential | 2.6 kg CO2 eq./kg |
| 5.7 kg CO2 eq./kg |
| 5.8kg CO2 eq./kg |
Land use (ReCiPe 2016) | 0.3 Annual crop eq. y |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.