MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

ExxonMobil HTA 002 High Density Polyethylene Resin
Categories: Polymer; Thermoplastic; Polyethylene (PE); High Density (HDPE)

Material Notes: Product Description: HTA 002 is a general purpose medium molecular weight HDPE grade, characterized by easy processability, especially in coextrusion and blending with other polyolefins. HTA 002 can also be used pure, especially for easy processing and conversion into small and thin bags, to be used for light item packaging.

Availability: Africa & Middle East, Asia Pacific and Europe

Additive:

  • Antiblock: No
  • Slip: No
  • Thermal Stabilizer: Yes
Applications:
  • Blown Film
  • Collation Shrink
  • Food packaging
  • General Packaging
  • Grocery Sacks
  • Heavy Duty Bags
  • Industrial Packaging
  • Label Film
  • Shrink Film
  • Stand Up Pouches
  • Thin Gauged Consumer Bags
  • Trash Bags
  • Trash Can Liners

Information provided by ExxonMobil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.952 g/cc0.0344 lb/in³ASTM D4883
Melt Flow 16 g/10 min
@Load 21.6 kg,
Temperature 190 °C
16 g/10 min
@Load 47.6 lb,
Temperature 374 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 29.0 MPa4200 psiASTM D882
Film Tensile Strength at Yield, TD 29.0 MPa4200 psiASTM D882
Film Elongation at Break, MD 320 %320 %ASTM D882
Film Elongation at Break, TD 450 %450 %ASTM D882
Elmendorf Tear Strength MD 8.0 g8.0 gASTM D1922
Elmendorf Tear Strength TD 60 g60 gASTM D1922
Dart Drop Test 160 g0.353 lbASTM D1709A
Film Tensile Strength at Break, MD 55.2 MPa8000 psiASTM D882
Film Tensile Strength at Break, TD 50.3 MPa7300 psiASTM D882
1% Secant Modulus, MD 965 MPa140000 psiASTM D882
1% Secant Modulus, TD 1170 MPa170000 psiASTM D882
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 126 °C259 °FASTM D1525

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ExxonMobil HMA 035 High Density Polyethylene Resin
ExxonMobil HD 6601.29 High Density Polyethylene Copolymer Resin
ExxonMobil AP60-007 High Density Polyethylene Resin
ExxonMobil AA48-002 High Density Polyethylene Resin
Total XT10B High Density Polyethylene, Pipe Resin

PEX99324 / 175560

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.