Physical Properties | Original Value | Comments |
---|
Density | 8.44 g/cc |
|
Mechanical Properties | Original Value | Comments |
---|
Tensile Strength, Ultimate | 905 MPa |
| 95.0 MPa @Temperature 1095 °C |
| 165 MPa @Temperature 980 °C |
| 345 MPa @Temperature 870 °C |
| 600 MPa @Temperature 760 °C |
| 760 MPa @Temperature 650 °C |
| 770 MPa @Temperature 540 °C |
Tensile Strength, Yield | 490 MPa @Strain 0.2 % |
| 39.0 MPa @Strain 0.2 %, Temperature 1095 °C |
| 83.0 MPa @Strain 0.2 %, Temperature 980 °C |
| 205 MPa @Strain 0.2 %, Temperature 870 °C |
| 345 MPa @Strain 0.2 %, Temperature 760 °C |
| 370 MPa @Strain 0.2 %, Temperature 540 °C |
| 370 MPa @Strain 0.2 %, Temperature 650 °C |
Elongation at Break | 48.5 % |
| 43.8 % @Temperature 980 °C |
| 44.7 % @Temperature 1095 °C |
| 45.9 % @Temperature 870 °C |
| 53.1 % @Temperature 760 °C |
| 54 % @Temperature 540 °C |
| 55.6 % @Temperature 650 °C |
Modulus of Elasticity | 208 GPa |
| 126 GPa @Temperature 1000 °C |
| 142 GPa @Temperature 900 °C |
| 153 GPa @Temperature 800 °C |
| 163 GPa @Temperature 700 °C |
| 171 GPa @Temperature 600 °C |
| 179 GPa @Temperature 500 °C |
| 186 GPa @Temperature 400 °C |
| 192 GPa @Temperature 300 °C |
| 199 GPa @Temperature 200 °C |
| 201 GPa @Temperature 100 °C |
|
Electrical Properties | Original Value | Comments |
---|
Electrical Resistivity | 0.000129 ohm-cm |
| 0.000132 ohm-cm @Temperature 100 °C |
| 0.000134 ohm-cm @Temperature 200 °C |
| 0.000135 ohm-cm @Temperature 300 °C |
| 0.000135 ohm-cm @Temperature 1000 °C |
| 0.000136 ohm-cm @Temperature 900 °C |
| 0.000136 ohm-cm @Temperature 400 °C |
| 0.000137 ohm-cm @Temperature 500 °C |
| 0.000137 ohm-cm @Temperature 800 °C |
| 0.000138 ohm-cm @Temperature 600 °C |
| 0.000138 ohm-cm @Temperature 700 °C |
|
Thermal Properties | Original Value | Comments |
---|
CTE, linear | 12.8 µm/m-°C @Temperature 25.0 - 100 °C |
| 13.1 µm/m-°C @Temperature 25.0 - 200 °C |
| 13.4 µm/m-°C @Temperature 25.0 - 300 °C |
| 13.8 µm/m-°C @Temperature 25.0 - 400 °C |
| 14.2 µm/m-°C @Temperature 25.0 - 500 °C |
| 14.8 µm/m-°C @Temperature 25.0 - 600 °C |
| 15.4 µm/m-°C @Temperature 25.0 - 700 °C |
| 16.0 µm/m-°C @Temperature 25.0 - 800 °C |
| 16.7 µm/m-°C @Temperature 25.0 - 900 °C |
| 17.4 µm/m-°C @Temperature 25.0 - 1000 °C |
Specific Heat Capacity | 0.410 J/g-°C |
| 0.428 J/g-°C @Temperature 100 °C |
| 0.455 J/g-°C @Temperature 200 °C |
| 0.477 J/g-°C @Temperature 300 °C |
| 0.503 J/g-°C @Temperature 400 °C |
| 0.527 J/g-°C @Temperature 500 °C |
| 0.552 J/g-°C @Temperature 600 °C |
| 0.576 J/g-°C @Temperature 700 °C |
| 0.600 J/g-°C @Temperature 800 °C |
| 0.625 J/g-°C @Temperature 900 °C |
| 0.648 J/g-°C @Temperature 1000 °C |
Thermal Conductivity | 9.80 W/m-K |
| 10.9 W/m-K @Temperature 100 °C |
| 12.5 W/m-K @Temperature 200 °C |
| 13.9 W/m-K @Temperature 300 °C |
| 15.3 W/m-K @Temperature 400 °C |
| 16.9 W/m-K @Temperature 500 °C |
| 18.3 W/m-K @Temperature 600 °C |
| 19.8 W/m-K @Temperature 700 °C |
| 21.5 W/m-K @Temperature 800 °C |
| 23.4 W/m-K @Temperature 900 °C |
| 25.6 W/m-K @Temperature 1000 °C |
Melting Point | 1290 - 1350 °C |
Solidus | 1290 °C |
Liquidus | 1350 °C |
|
Component Elements Properties | Original Value | Comments |
---|
Aluminum, Al | <= 0.40 % |
Carbon, C | <= 0.10 % |
Chromium, Cr | 21 % |
Cobalt, Co | <= 1.0 % |
Iron, Fe | <= 5.0 % |
Manganese, Mn | <= 0.50 % |
Molybdenum, Mo | 9.0 % |
Nickel, Ni | 62 % |
Niobium, Nb (Columbium, Cb) | 3.7 % |
Silicon, Si | <= 0.50 % |
Titanium, Ti | <= 0.40 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to go back to viewing the property data in MatWeb's normal format.