MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Haynes 625 alloy, cold rolled and 1050°C mill-annealed sheet
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Excellent strength up to 816°C, good oxidation resistance and aqueous corrosion, excellent forming and welding characteristics. Applications include a variety of high-temperature aerospace, chemical process industry and power industry uses. Widely used in sea water and power plant scrubber applications.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: ASTM B444, ASTM B446, ASTM B704, ASTM B705, ASTM B366, AWS A5.14, UNS N06625, AMS 5599, AMS 5666, AMS 5837, ASTM B443
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.44 g/cc0.305 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 905 MPa131000 psi
 95.0 MPa
@Temperature 1095 °C
13800 psi
@Temperature 2003 °F
 165 MPa
@Temperature 980 °C
23900 psi
@Temperature 1800 °F
 345 MPa
@Temperature 870 °C
50000 psi
@Temperature 1600 °F
 600 MPa
@Temperature 760 °C
87000 psi
@Temperature 1400 °F
 760 MPa
@Temperature 650 °C
110000 psi
@Temperature 1200 °F
 770 MPa
@Temperature 540 °C
112000 psi
@Temperature 1000 °F
Tensile Strength, Yield 490 MPa
@Strain 0.2 %
71100 psi
@Strain 0.2 %
 39.0 MPa
@Strain 0.2 %,
Temperature 1095 °C
5660 psi
@Strain 0.2 %,
Temperature 2003 °F
 83.0 MPa
@Strain 0.2 %,
Temperature 980 °C
12000 psi
@Strain 0.2 %,
Temperature 1800 °F
 205 MPa
@Strain 0.2 %,
Temperature 870 °C
29700 psi
@Strain 0.2 %,
Temperature 1600 °F
 345 MPa
@Strain 0.2 %,
Temperature 760 °C
50000 psi
@Strain 0.2 %,
Temperature 1400 °F
 370 MPa
@Strain 0.2 %,
Temperature 540 °C
53700 psi
@Strain 0.2 %,
Temperature 1000 °F
 370 MPa
@Strain 0.2 %,
Temperature 650 °C
53700 psi
@Strain 0.2 %,
Temperature 1200 °F
Elongation at Break 48.5 %48.5 %in 50.8 mm
 43.8 %
@Temperature 980 °C
43.8 %
@Temperature 1800 °F
in 50.8 mm
 44.7 %
@Temperature 1095 °C
44.7 %
@Temperature 2003 °F
in 50.8 mm
 45.9 %
@Temperature 870 °C
45.9 %
@Temperature 1600 °F
in 50.8 mm
 53.1 %
@Temperature 760 °C
53.1 %
@Temperature 1400 °F
in 50.8 mm
 54 %
@Temperature 540 °C
54 %
@Temperature 1000 °F
in 50.8 mm
 55.6 %
@Temperature 650 °C
55.6 %
@Temperature 1200 °F
in 50.8 mm
Modulus of Elasticity 208 GPa30200 ksiRT
 126 GPa
@Temperature 1000 °C
18300 ksi
@Temperature 1830 °F
 142 GPa
@Temperature 900 °C
20600 ksi
@Temperature 1650 °F
 153 GPa
@Temperature 800 °C
22200 ksi
@Temperature 1470 °F
 163 GPa
@Temperature 700 °C
23600 ksi
@Temperature 1290 °F
 171 GPa
@Temperature 600 °C
24800 ksi
@Temperature 1110 °F
 179 GPa
@Temperature 500 °C
26000 ksi
@Temperature 932 °F
 186 GPa
@Temperature 400 °C
27000 ksi
@Temperature 752 °F
 192 GPa
@Temperature 300 °C
27800 ksi
@Temperature 572 °F
 199 GPa
@Temperature 200 °C
28900 ksi
@Temperature 392 °F
 201 GPa
@Temperature 100 °C
29200 ksi
@Temperature 212 °F
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000129 ohm-cm0.000129 ohm-cmRT
 0.000132 ohm-cm
@Temperature 100 °C
0.000132 ohm-cm
@Temperature 212 °F
 0.000134 ohm-cm
@Temperature 200 °C
0.000134 ohm-cm
@Temperature 392 °F
 0.000135 ohm-cm
@Temperature 300 °C
0.000135 ohm-cm
@Temperature 572 °F
 0.000135 ohm-cm
@Temperature 1000 °C
0.000135 ohm-cm
@Temperature 1830 °F
 0.000136 ohm-cm
@Temperature 900 °C
0.000136 ohm-cm
@Temperature 1650 °F
 0.000136 ohm-cm
@Temperature 400 °C
0.000136 ohm-cm
@Temperature 752 °F
 0.000137 ohm-cm
@Temperature 500 °C
0.000137 ohm-cm
@Temperature 932 °F
 0.000137 ohm-cm
@Temperature 800 °C
0.000137 ohm-cm
@Temperature 1470 °F
 0.000138 ohm-cm
@Temperature 600 °C
0.000138 ohm-cm
@Temperature 1110 °F
 0.000138 ohm-cm
@Temperature 700 °C
0.000138 ohm-cm
@Temperature 1290 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.8 µm/m-°C
@Temperature 25.0 - 100 °C
7.11 µin/in-°F
@Temperature 77.0 - 212 °F
 13.1 µm/m-°C
@Temperature 25.0 - 200 °C
7.28 µin/in-°F
@Temperature 77.0 - 392 °F
 13.4 µm/m-°C
@Temperature 25.0 - 300 °C
7.44 µin/in-°F
@Temperature 77.0 - 572 °F
 13.8 µm/m-°C
@Temperature 25.0 - 400 °C
7.67 µin/in-°F
@Temperature 77.0 - 752 °F
 14.2 µm/m-°C
@Temperature 25.0 - 500 °C
7.89 µin/in-°F
@Temperature 77.0 - 932 °F
 14.8 µm/m-°C
@Temperature 25.0 - 600 °C
8.22 µin/in-°F
@Temperature 77.0 - 1110 °F
 15.4 µm/m-°C
@Temperature 25.0 - 700 °C
8.56 µin/in-°F
@Temperature 77.0 - 1290 °F
 16.0 µm/m-°C
@Temperature 25.0 - 800 °C
8.89 µin/in-°F
@Temperature 77.0 - 1470 °F
 16.7 µm/m-°C
@Temperature 25.0 - 900 °C
9.28 µin/in-°F
@Temperature 77.0 - 1650 °F
 17.4 µm/m-°C
@Temperature 25.0 - 1000 °C
9.67 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.410 J/g-°C0.0980 BTU/lb-°FRT
 0.428 J/g-°C
@Temperature 100 °C
0.102 BTU/lb-°F
@Temperature 212 °F
 0.455 J/g-°C
@Temperature 200 °C
0.109 BTU/lb-°F
@Temperature 392 °F
 0.477 J/g-°C
@Temperature 300 °C
0.114 BTU/lb-°F
@Temperature 572 °F
 0.503 J/g-°C
@Temperature 400 °C
0.120 BTU/lb-°F
@Temperature 752 °F
 0.527 J/g-°C
@Temperature 500 °C
0.126 BTU/lb-°F
@Temperature 932 °F
 0.552 J/g-°C
@Temperature 600 °C
0.132 BTU/lb-°F
@Temperature 1110 °F
 0.576 J/g-°C
@Temperature 700 °C
0.138 BTU/lb-°F
@Temperature 1290 °F
 0.600 J/g-°C
@Temperature 800 °C
0.143 BTU/lb-°F
@Temperature 1470 °F
 0.625 J/g-°C
@Temperature 900 °C
0.149 BTU/lb-°F
@Temperature 1650 °F
 0.648 J/g-°C
@Temperature 1000 °C
0.155 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 9.80 W/m-K68.0 BTU-in/hr-ft²-°FRT
 10.9 W/m-K
@Temperature 100 °C
75.6 BTU-in/hr-ft²-°F
@Temperature 212 °F
 12.5 W/m-K
@Temperature 200 °C
86.8 BTU-in/hr-ft²-°F
@Temperature 392 °F
 13.9 W/m-K
@Temperature 300 °C
96.5 BTU-in/hr-ft²-°F
@Temperature 572 °F
 15.3 W/m-K
@Temperature 400 °C
106 BTU-in/hr-ft²-°F
@Temperature 752 °F
 16.9 W/m-K
@Temperature 500 °C
117 BTU-in/hr-ft²-°F
@Temperature 932 °F
 18.3 W/m-K
@Temperature 600 °C
127 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 19.8 W/m-K
@Temperature 700 °C
137 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 21.5 W/m-K
@Temperature 800 °C
149 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 23.4 W/m-K
@Temperature 900 °C
162 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 25.6 W/m-K
@Temperature 1000 °C
178 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1290 - 1350 °C2350 - 2460 °F
Solidus 1290 °C2350 °F
Liquidus 1350 °C2460 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al <= 0.40 %<= 0.40 %
Carbon, C <= 0.10 %<= 0.10 %
Chromium, Cr 21 %21 %
Cobalt, Co <= 1.0 %<= 1.0 %
Iron, Fe <= 5.0 %<= 5.0 %
Manganese, Mn <= 0.50 %<= 0.50 %
Molybdenum, Mo 9.0 %9.0 %
Nickel, Ni 62 %62 %As Remainder
Niobium, Nb (Columbium, Cb) 3.7 %3.7 %Includes Ta
Silicon, Si <= 0.50 %<= 0.50 %
Titanium, Ti <= 0.40 %<= 0.40 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Type 904L Austenitic Stainless Steel, Annealed Plate, Sheet, Strip, UNS N08904
Special Metals INCONEL® Alloy 625
ATI Allvac® Nickelvac® 625 Nickel Superalloy, Heat Treatment: 927°C (1700°F) Anneal
ATI Allegheny Ludlum Stainless Steel AL-6XN® Alloy (UNS N08367)
Haynes 625 alloy, hot rolled and 1050°C mill-annealed plate

NH62AA / 16716

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.