MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Carpenter Custom 455® Stainless Steel, Condition H900 (Age Hardened 482°C)
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: Data provided by Carpenter Technology Corporation.

Recognizing the need for high-strength alloys with good corrosion resistance to atmospheric environments, the Carpenter Research Laboratory developed Custom 455® stainless, a martensitic age-hardenable stainless steel. This alloy is relatively soft and formable in the annealed condition. A single-step aging treatment develops exceptionally high yield strength with good ductility and toughness. This stainless can be machined in the annealed condition, and welded in much the same manner as other precipitation hardenable stainless steels. Because of its low work-hardening rate, it can be extensively cold formed. The dimensional change during hardening is only about -0.001 in/in, which permits close-tolerance finish machining in the annealed state. Custom 455 stainless represents a significant advancement in the area of precipitation hardening stainless steels. It should be considered where simplicity of heat treatment, ease of fabrication, high strength and corrosion resistance are required in combination.

Because of the unique combination of high strength and corrosion resistance of Custom 455 stainless there are few other alloys available for consideration. Carpenter PH13-8 Mo can be considered where good transverse toughness and ductility are necessary in large sections.

Custom 455® is a registered trademark of Carpenter Technology Corporation.

Key Words: UNS S45500
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 7.76 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 472Estimated from Rockwell C for Brinell test with 3000 kg load, 10 mm ball.
Hardness, Knoop 519Estimated from Rockwell C
Hardness, Rockwell C 49
Hardness, Vickers 496Estimated from Rockwell C
Tensile Strength, Ultimate 1689 MPa
 1241 MPa
@Temperature 427 °C
 1345 MPa
@Temperature 371 °C
 1407 MPa
@Temperature 316 °C
 1476 MPa
@Temperature 260 °C
Tensile Strength, Yield 1634 MPa
@Strain 0.2 %
 1145 MPa
@Strain 0.2 %,
Temperature 427 °C
 1241 MPa
@Strain 0.2 %,
Temperature 371 °C
 1296 MPa
@Strain 0.2 %,
Temperature 316 °C
 1372 MPa
@Strain 0.2 %,
Temperature 260 °C
Elongation at Break 11 %In 4D
 10 %
@Temperature 260 °C
In 4D
 12 %
@Temperature 371 °C
In 4D
 14 %
@Temperature 427 °C
In 4D
Reduction of Area 48 %
 49 %
@Temperature 260 °C
 50 %
@Temperature 316 °C
 52 %
@Temperature 371 °C
 56 %
@Temperature 427 °C
Modulus of Elasticity 200 GPa
Poissons Ratio 0.30
@Temperature 23.0 °C
Fatigue Strength 772 MPa
@# of Cycles 1.00e+7
R.R. Moore Test, Smooth Rotating Beam
Shear Modulus 76.9 GPa
@Temperature 23.0 °C
Charpy Impact 12.0 J
@Diameter 25.0 mm
bar
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.0000758 ohm-cm
@Temperature 23.0 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 10.6 µm/m-°C
@Temperature 22.0 - 93.0 °C
 11.2 µm/m-°C
@Temperature 22.0 - 260 °C
 12.0 µm/m-°C
@Temperature 22.0 - 482 °C
 
Component Elements PropertiesOriginal ValueComments
Carbon, C <= 0.050 %
Chromium, Cr 11 - 12.5 %
Copper, Cu 1.5 - 2.5 %
Iron, Fe 75 %as remainder
Manganese, Mn <= 0.50 %
Molybdenum, Mo <= 0.50 %
Nb + Ta 0.10 - 0.50 %
Nickel, Ni 7.5 - 9.5 %
Niobium, Nb (Columbium, Cb) <= 0.50 %
Phosphorus, P <= 0.040 %
Silicon, Si <= 0.50 %
Sulfur, S <= 0.030 %
Tantalum, Ta <= 0.50 %
Titanium, Ti 0.80 - 1.4 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Carpenter Custom 455® Stainless Steel, Condition H1000 (Age Hardened 538°C (1000°F))
Carpenter Custom 455® Stainless Steel, Condition H950 (Age Hardened 510°C)
Carpenter Custom 455® Stainless Steel, Annealed, 25 mm Bar
Carpenter Custom 455® Stainless Steel, Annealed, 1.27 mm Strip
AK Steel 17-4 PH® Precipitation Hardening Stainless Steel, Condition H 900

NCAR72 / 15638

New MatWeb Services

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.