MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Dow VERSIFY™ 2000 Plastomer
Categories: Polymer; Thermoplastic; Adhesives, Sealants, and Coatings

Material Notes: VERSIFY™ 2000 Plastomer is a resin with a low melt flow rate making it suitable for blown film, blow molding, extrusion and thermoforming. It is an excellent sealant and is particularly suitable for use in BOPE structures. It has excellent compatibility with PP and is useful agent to bring softness and temperature performance.

Main Characteristics:

  • Pellet
  • Low Melt Flow Rate
  • Good sealant
  • Compatible with PP
  • Soft polypropylene
Applications:
  • Blown Film
  • Sealant
  • BOPE
  • Extrusion Applications
Complies with
  • EU, No 10/2011
  • US FDA FCN 909
  • US FDA 21 CFR 175.105(c)(5)
Consult the regulations for complete details.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.888 g/cc0.0321 lb/in³ASTM D792
Melt Index of Compound 2.0 g/10 min
@Load 2.16 kg,
Temperature 230 °C
2.0 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
Crystallinity 35 %35 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 96
@Time 10.0 sec
96
@Time 0.00278 hour
Compression Molded; ASTM D2240
Hardness, Shore D 54
@Time 10.0 sec
54
@Time 0.00278 hour
Compression Molded; ASTM D2240
Tensile Strength at Break 26.0 MPa3770 psiCompression Molded; ASTM D638
Elongation at Break 680 %680 %50 mm/min, Compression Molded; ASTM D638
Flexural Modulus 0.359 GPa
@Strain 2 %
52.1 ksi
@Strain 2 %
Aged two weeks, Secant (Compression Molded); ASTM D790
 
Thermal PropertiesMetricEnglishComments
Melting Point 107 °C225 °FDSC
Vicat Softening Point 94.0 °C201 °FASTM D1525
Glass Transition Temp, Tg -17.0 °C1.40 °FDSC
 
Optical PropertiesMetricEnglishComments
Haze 18 %
@Thickness 2.00 mm
18 %
@Thickness 0.0787 in
Injection Molded; ASTM D1003
Gloss  108 %
@Thickness 1.00 mm
108 %
@Thickness 0.0394 in
20°, Compression Molded, Gardner; ASTM D523
 119 %
@Thickness 1.00 mm
119 %
@Thickness 0.0394 in
60°, Compression Molded, Gardner; ASTM D523
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow VERSIFY™ 2200 Plastomer
Dow VERSIFY™ 2300 Elastomer
Dow VERSIFY™ 3000 Plastomer
Dow VERSIFY™ 3200 Elastomer
Dow VERSIFY™ 3300 Elastomer

PDOW2033 / 183680

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.