MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

3M Techical Ceramics MYCROSINT® CD Boron Nitride
Categories: Ceramic; Carbide

Material Notes:

Information provided by 3M Technical Ceramics, formerly ESK Ceramics.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density >= 1.97 g/cc>= 0.0712 lb/in³Anisotropic, Perpendicular; DIN EN 623-2
 >= 1.97 g/cc>= 0.0712 lb/in³Anisotropic, Parallel; DIN EN 623-2
Porosity <= 12 %<= 12 %Anisotropic, Perpendicular; DIN EN 623-2
 <= 12 %<= 12 %Anisotropic, Parallel; DIN EN 623-2
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 1313Anisotropic, Perpendicular; DIN EN ISO 6506-1
 1313Anisotropic, Parallel; DIN EN ISO 6506-1
Tensile Modulus 25.0 GPa3630 ksiYoung's, Anisotropic, Parallel; DIN EN 843-2
 30.0 GPa4350 ksiYoung's, Anisotropic, Perpendicular; DIN EN 843-2
Flexural Strength 35.0 MPa5080 psiAnisotropic, Parallel; DIN EN 843-1
 40.0 MPa5800 psiAnisotropic, Perpendicular; DIN EN 843-1
Compressive Strength 50.0 MPa7250 psiAnisotropic, Perpendicular; AAW/AC-R-302-03
 55.0 MPa7980 psiAnisotropic, Parallel; AAW/AC-R-302-03
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity >= 1.00e+12 ohm-cm>= 1.00e+12 ohm-cmAnisotropic, Perpendicular
 >= 1.00e+12 ohm-cm>= 1.00e+12 ohm-cmAnisotropic, Parallel
 
Thermal PropertiesMetricEnglishComments
CTE, linear  -1.00 µm/m-°C
@Temperature 20.0 - 500 °C
-0.556 µin/in-°F
@Temperature 68.0 - 932 °F
Anisotropic, Perpendicular; DIN EN 821-1
 -1.00 µm/m-°C
@Temperature 20.0 - 500 °C
-0.556 µin/in-°F
@Temperature 68.0 - 932 °F
Anisotropic, Parallel; DIN EN 821-1
 1.50 µm/m-°C
@Temperature 500 - 1000 °C
0.833 µin/in-°F
@Temperature 932 - 1830 °F
Anisotropic, Perpendicular; DIN EN 821-1
 2.00 µm/m-°C
@Temperature 500 - 1000 °C
1.11 µin/in-°F
@Temperature 932 - 1830 °F
Anisotropic, Parallel; DIN EN 821-1
 3.00 µm/m-°C
@Temperature 1000 - 1500 °C
1.67 µin/in-°F
@Temperature 1830 - 2730 °F
Anisotropic, Perpendicular; DIN EN 821-1
 4.00 µm/m-°C
@Temperature 1000 - 1500 °C
2.22 µin/in-°F
@Temperature 1830 - 2730 °F
Anisotropic, Parallel; DIN EN 821-1
Specific Heat Capacity 0.580 J/g-°C0.139 BTU/lb-°FAnisotropic, Perpendicular
 0.580 J/g-°C0.139 BTU/lb-°FAnisotropic, Parallel
Thermal Conductivity 35.0 W/m-K243 BTU-in/hr-ft²-°FAnisotropic, Perpendicular
 35.0 W/m-K243 BTU-in/hr-ft²-°FAnisotropic, Parallel
Maximum Service Temperature, Air 1100 °C2010 °FOxidizing, Anisotropic, Perpendicular
 1100 °C2010 °FOxidizing, Anisotropic, Parallel
Maximum Service Temperature, Inert 1500 °C2730 °FAnisotropic, Perpendicular
 1500 °C2730 °FAnisotropic, Parallel

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Momentive Performance Materials HBR Hot-Pressed Boron Nitride
Silicon Carbide, Reaction-Bonded, SiSiC
Thermal Transfer Composites PRIMEX ULTRA™ MCT-587™ Aluminum Silicon Carbide Composite, Reinforced
3M Techical Ceramics MYCROSINT® HD Boron Nitride
CoorsTek Reaction Bonded Silicon Carbide, SCRB (SC-2)

CESK16 / 183308

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.