MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

AISI 1016 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round
Categories: Metal; Ferrous Metal; Carbon Steel; AISI 1000 Series Steel; Low Carbon Steel

Material Notes: Most widely used in cold forming operations such as heading, upsetting, and extrusion.

Key Words: UNS G10160, ASTM A29, ASTM A108, ASTM A510, ASTM A513, ASTM A545, carbon steels, ASTM A548, ASTM A549, ASTM A576, ASTM A659, MIL SPEC MIL-S-866, SAE J403, SAE J412, SAE J414, DIN 1.0419, DIN 1.1142, DIN GS-Ck16, DIN RSt44.2, DIN 17115 1.0467, DIN 17115 1.0468, DIN 17115 15Mn3, DIN 17115 15Mn3Al, BS 3059 440, BS 3606 440, BS 970 080A15, BS 970 080M15, BS 970 170H15, BS 970 173H16, EN32, AISI1016
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.87 g/cc0.284 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 121121
Hardness, Knoop 140140Converted from Brinell
Hardness, Rockwell B 6868Converted from Brinell
Hardness, Vickers 126126Converted from Brinell
Tensile Strength, Ultimate 420 MPa60900 psi
Tensile Strength, Yield 350 MPa50800 psi
Elongation at Break 18 %18 %In 50 mm
Reduction of Area 40 %40 %
Modulus of Elasticity 205 GPa29700 ksiTypical for steel
Bulk Modulus 160 GPa23200 ksiTypical for steel
Poissons Ratio 0.290.29Typical For Steel
Machinability 70 %70 %Based on AISI 1212 steel = 100%
Shear Modulus 80.0 GPa11600 ksiTypical for steel
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity  0.0000160 ohm-cm
@Temperature 0.000 °C
0.0000160 ohm-cm
@Temperature 32.0 °F
annealed condition
 0.0000220 ohm-cm
@Temperature 100 °C
0.0000220 ohm-cm
@Temperature 212 °F
annealed condition
 0.0000290 ohm-cm
@Temperature 200 °C
0.0000290 ohm-cm
@Temperature 392 °F
annealed condition
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity  0.481 J/g-°C
@Temperature >=100 °C
0.115 BTU/lb-°F
@Temperature >=212 °F
annealed
 0.515 J/g-°C
@Temperature 150 - 200 °C
0.123 BTU/lb-°F
@Temperature 302 - 392 °F
 0.595 J/g-°C
@Temperature 350 - 400 °C
0.142 BTU/lb-°F
@Temperature 662 - 752 °F
Thermal Conductivity 51.9 W/m-K360 BTU-in/hr-ft²-°Festimated based on similar materials
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.12 - 0.18 %0.12 - 0.18 %
Iron, Fe 99.13 - 99.58 %99.13 - 99.58 %As remainder
Manganese, Mn 0.60 - 0.90 %0.60 - 0.90 %
Phosphorus, P <= 0.040 %<= 0.040 %
Sulfur, S <= 0.050 %<= 0.050 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
AISI 1016 Steel, hot rolled, 19-32 mm (0.75-1.25 in) round
AISI 1017 Steel, cold drawn
AISI 1018 Steel, cold drawn
AISI 1010 Steel, cold drawn bar, 19-32 mm (0.75-1.25 in) round or thickness
AISI 1018 Steel, as cold drawn, 16-22 mm (0.625-0.875 in) round

M1016A / 6805

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.