MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Trinseo Magnum™ 1150 EM Acrylonitrile Butadiene Styrene (ABS)
Categories: Polymer; Thermoplastic; ABS Polymer

Material Notes: MAGNUM™ ABS resins are thermoplastic material which provide an excellent balance of processability, impact resistance and heat resistance as imparted by the various polymer compositions. MAGNUM ABS resin are available in a wide range of melt flow rates, impact strength and heat resistance for both high and low gloss applications manufactured by injection molding, sheet or profile extrusion and thermoforming processes. The automotive grades of MAGNUM ABS resins offer a wide range of gloss, viscosities, impact strength and heat properties for use in numerous automotive applications. Melt flow rates from 1 to 12 g/10 min, impact strengths from 2.5 to 12 ft-lb/in and heat distortion temperatures from 165 to 190°F are available. Available primarily as natural plus concentrates, MAGNUM ABS resins are used in a wide variety of automotive applications including structural instrument panels, consoles, pillars and exterior trim parts requiring painting and plating. Within the MAGNUM ABS product line, MAGNUM 1150 EM ABS resin is a high impact, medium heat, low gloss resin. MAGNUM™ 1150 EM has improved low temperature impact strength over standard grades of ABS. MAGNUM™ 1150 EM is used in applications like pillars and instrument panel trim.

Automotive Specifications:

  • CHRYSLER MS-DB-198 Type B CPN3903 Color: 100% Color Match

Information provided by Trinseo.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.03 g/cc0.0372 lb/in³ASTM D792
Linear Mold Shrinkage, Flow 0.0060 - 0.0070 cm/cm0.0060 - 0.0070 in/inASTM D955
Melt Flow 0.90 g/10 min
@Load 3.80 kg,
Temperature 230 °C
0.90 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 36.5 MPa
@Thickness 3.20 mm
5290 psi
@Thickness 0.126 in
51 mm/min; ASTM D638
Elongation at Break 30 %
@Thickness 3.20 mm
30 %
@Thickness 0.126 in
51 mm/min; ASTM D638
Elongation at Yield 3.0 %
@Thickness 3.20 mm
3.0 %
@Thickness 0.126 in
51 mm/min; ASTM D638
Tensile Modulus 1.75 GPa
@Thickness 3.20 mm
254 ksi
@Thickness 0.126 in
51 mm/min; ASTM D638
Flexural Strength 58.9 MPa
@Thickness 3.20 mm
8540 psi
@Thickness 0.126 in
5.1 mm/min; ASTM D790
Flexural Modulus 1.98 GPa287 ksi5.1 mm/min; ASTM D790
Izod Impact, Notched  3.40 J/cm
@Thickness 3.20 mm,
Temperature -29.0 °C
6.37 ft-lb/in
@Thickness 0.126 in,
Temperature -20.2 °F
ASTM D256
 5.60 J/cm
@Thickness 3.20 mm,
Temperature 23.0 °C
10.5 ft-lb/in
@Thickness 0.126 in,
Temperature 73.4 °F
ASTM D256
Dart Drop, Total Energy  29.9 J
@Thickness 3.20 mm,
Temperature 23.0 °C
22.1 ft-lb
@Thickness 0.126 in,
Temperature 73.4 °F
Peak, 6.71 m/sec; ASTM D3763
 32.8 J
@Thickness 3.20 mm,
Temperature -29.0 °C
24.2 ft-lb
@Thickness 0.126 in,
Temperature -20.2 °F
Peak, 6.71 m/sec; ASTM D3763
 42.9 J
@Thickness 3.20 mm,
Temperature -29.0 °C
31.6 ft-lb
@Thickness 0.126 in,
Temperature -20.2 °F
6.71 m/sec; ASTM D3763
 45.2 J
@Thickness 3.20 mm,
Temperature 23.0 °C
33.3 ft-lb
@Thickness 0.126 in,
Temperature 73.4 °F
6.71 m/sec; ASTM D3763
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 95.0 µm/m-°C
@Thickness 3.20 mm
52.8 µin/in-°F
@Thickness 0.126 in
ASTM D969
Deflection Temperature at 0.46 MPa (66 psi)  96.1 °C
@Thickness 3.20 mm
205 °F
@Thickness 0.126 in
Unannealed; ASTM D648
 111 °C
@Thickness 3.20 mm
232 °F
@Thickness 0.126 in
Annealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi)  82.2 °C
@Thickness 3.20 mm
180 °F
@Thickness 0.126 in
Unannealed; ASTM D648
 108 °C
@Thickness 3.20 mm
226 °F
@Thickness 0.126 in
Annealed; ASTM D648
Vicat Softening Point 112 °C234 °FASTM D1525
 
Processing PropertiesMetricEnglishComments
Melt Temperature 218 - 274 °C424 - 525 °F
Mold Temperature 27.0 - 60.0 °C80.6 - 140 °F
Drying Temperature 82.0 °C180 °F
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hour
Back Pressure 1.03 - 3.45 MPa149 - 500 psi
Clamp Pressure 28.0 - 69.0 MPa4060 - 10000 psi
 
Descriptive Properties
Screw Compression Ratio1.5:1.0 to 3.5:1.0
Screw L/D Ratio20:1

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
A. Schulman Diamond TR 5000
Envalior Arnitel® EL250 TPC-ET, Injection Molding
Trinseo CALIBRE™ MEGARAD 2080 15 Polycarbonate, Gamma Radiation Resistant
Chevron Phillips EA3025 Crystal Polystyrene
Ineos ABS Centrex® 401 AES Extrusion

PDOW1396 / 30614

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.