MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

LyondellBasell Petrothene® GA808091 Linear Low Density Polyethylene
Categories: Polymer; Thermoplastic; Polyethylene (PE); Linear Low Density (LLDPE)

Material Notes: Applications
PETROTHENE GA 808-091 is a broad molecular weight, linear low density polyethylene resin designed for use as a base resin in wire and cable jacketing. An antioxidant package is added to ensure thermal stability during processing.

Processing Techniques
GA 808-091, like other thermoplastic polyolefin resins, can be extruded as wire and cable insulation using a conventional extruder. Below are suggested extrusion conditions for GA 808-091. These conditions are intended as general guidelines only and are not optimum values, since manufacturing conditions, such as extruder type and size have an effect on the processing of thermoplastic resins.

Industry Specifications
GA 808-091 meets the requirements of the following: ASTM D1248, Type 1, Category 4, Class A, Grade E5. Federal LP390C, Type II, Class L, Category 4, Grade 4.

This product is from the former Equistar product line.

Key Words: LLDPE;Fiber Optic/Coaxial General Purpose; Telecom/ Telecommunications; Natural Insulation; Jacketing Base
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.920 g/cc0.0332 lb/in³ASTM D1505
ESCR 10% Igepal® >= 1000 hour>= 1000 hourF50; ASTM D1693
Melt Flow 0.75 g/10 min0.75 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5757ASTM D2240
Tensile Strength at Break 15.2 MPa2200 psiASTM D638
Tensile Strength, Yield 11.7 MPa1700 psiASTM D638
Elongation at Break 650 %650 %ASTM D638
Flexural Modulus, 1% Secant 345 MPa50000 psiASTM D790
 
Electrical PropertiesMetricEnglishComments
Dielectric Constant 2.292.29ASTM D1531
Dissipation Factor 0.0000600.000060ASTM D1531
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature <= -76.0 °C<= -105 °FF50; ASTM D746
 
Processing PropertiesMetricEnglishComments
Feed Temperature 154 - 163 °C310 - 325 °F
Zone 2 177 - 193 °C350 - 380 °F
Zone 3 193 - 210 °C380 - 410 °F
Zone 4-x 204 - 218 °C400 - 425 °F
Adapter Temperature 204 - 218 °C400 - 425 °F
Die Temperature 204 - 218 °C400 - 425 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
LyondellBasell Petrothene® NA217080 Low Density Polyethylene
LyondellBasell Petrothene® LR590001 High Density Polyethylene
LyondellBasell Alathon® M5370WC High Density Polyethylene
LyondellBasell Microthene® MP564189 Linear Low Density Polyethylene, Injection Molding Grade
LyondellBasell Microthene® MP574189 Linear Low Density Polyethylene, Injection Molding Grade

PEQU0391 / 36834

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.