MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Covestro Texin® 985 Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 985 resin is an aromatic polyether-based thermoplastic polyurethane with a Shore hardness of approximately 85A. It can be processed by injection molding, extrusion, or blow molding.

Properties / Applications: Texin 985 resin offers outstanding abrasion resistance, impact strength, toughness, and flexibility. It also exhibits excellent inherent resistance to salt water stress cracking, and hydrolysis. Texin 985 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. In addition, Texin 985 natural color resin is listed under NSF standard 61 for use in potable water applications. Typical applications include gaskets, hose, tubing, shoe inserts, connectors, belting, and miscellaneous molded articles.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.12 g/cc1.12 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
0.0080 in/in
@Thickness 0.100 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 8585ASTM D2240
 76
@Time 1.81e+6 sec
76
@Time 504 hour
Fuel C; ASTM D471
 77
@Time 252000 sec
77
@Time 70.0 hour
Fuel C; ASTM D471
 77
@Time 605000 sec
77
@Time 168 hour
Fuel C; ASTM D471
 83
@Time 252000 sec
83
@Time 70.0 hour
Fuel A; ASTM D471
 84
@Time 605000 sec
84
@Time 168 hour
Fuel A; ASTM D471
 84
@Time 1.81e+6 sec
84
@Time 504 hour
Fuel A; ASTM D471
 85
@Time 1.21e+6 sec
85
@Time 336 hour
Fuel A; ASTM D471
 85
@Time 1.21e+6 sec
85
@Time 336 hour
Fuel C; ASTM D471
 70
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
70
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 71
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
71
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
 72
@Treatment Temp. 100 °C,
Time 605000 sec
72
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
 75
@Treatment Temp. 100 °C,
Time 252000 sec
75
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 76
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
76
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 77
@Treatment Temp. 100 °C,
Time 252000 sec
77
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 77
@Treatment Temp. 100 °C,
Time 605000 sec
77
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 78
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
78
@Treatment Temp. 257 °F,
Time 336 hour
Hot Air; ASTM D573
 78
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
78
@Treatment Temp. 257 °F,
Time 504 hour
Hot Air; ASTM D573
 80
@Treatment Temp. 125 °C,
Time 252000 sec
80
@Treatment Temp. 257 °F,
Time 70.0 hour
Hot Air; ASTM D573
 80
@Treatment Temp. 100 °C,
Time 605000 sec
80
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 80
@Treatment Temp. 125 °C,
Time 605000 sec
80
@Treatment Temp. 257 °F,
Time 168 hour
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 252000 sec
81
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
81
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
81
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
Tensile Strength at Break 38.6 MPa5600 psiASTM D412
 19.3 MPa
@Time 1.21e+6 sec
2800 psi
@Time 336 hour
Fuel C; ASTM D471
 23.932 MPa
@Time 252000 sec
3471.0 psi
@Time 70.0 hour
Fuel C; ASTM D471
 24.704 MPa
@Time 1.81e+6 sec
3583.0 psi
@Time 504 hour
Fuel C; ASTM D471
 25.476 MPa
@Time 605000 sec
3695.0 psi
@Time 168 hour
Fuel C; ASTM D471
 37.056 MPa
@Time 252000 sec
5374.5 psi
@Time 70.0 hour
Fuel A; ASTM D471
 39.758 MPa
@Time 605000 sec
5766.4 psi
@Time 168 hour
Fuel A; ASTM D471
 43.223 MPa
@Time 1.21e+6 sec
6269.0 psi
@Time 336 hour
Fuel A; ASTM D471
 43.618 MPa
@Time 1.81e+6 sec
6326.3 psi
@Time 504 hour
Fuel A; ASTM D471
 11.58 MPa
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
1680 psi
@Treatment Temp. 257 °F,
Time 504 hour
Hot Air; ASTM D573
 12.738 MPa
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
1847.5 psi
@Treatment Temp. 257 °F,
Time 336 hour
Hot Air; ASTM D573
 16.212 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
2351.4 psi
@Treatment Temp. 257 °F,
Time 168 hour
Hot Air; ASTM D573
 21.616 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
3135.1 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
 24.318 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
3527.0 psi
@Treatment Temp. 257 °F,
Time 70.0 hour
Hot Air; ASTM D573
 27.02 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
3919 psi
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 27.792 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
4030.9 psi
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 29.336 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
4254.8 psi
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 29.722 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
4310.8 psi
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
 32.81 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
4759 psi
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
 35.512 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
5150.6 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 36.284 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
5262.6 psi
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 36.284 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
5262.6 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 39.758 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
5766.4 psi
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 40.144 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
5822.4 psi
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 41.302 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
5990.4 psi
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
Tensile Stress at Strain  4.40 MPa
@Strain 100 %
638 psi
@Strain 100 %
ASTM Oil #3, 70; ASTM D471
 4.40 MPa
@Strain 100 %
638 psi
@Strain 100 %
ASTM Oil #3, 504; ASTM D471
 4.62 MPa
@Strain 100 %
670 psi
@Strain 100 %
ASTM Oil #3, 336; ASTM D471
 4.80 MPa
@Strain 50 %
696 psi
@Strain 50 %
ASTM D412
 4.95 MPa
@Strain 100 %
718 psi
@Strain 100 %
ASTM Oil #3, 168; ASTM D471
 5.50 MPa
@Strain 100 %
798 psi
@Strain 100 %
ASTM D412
 9.312 MPa
@Strain 300 %
1351 psi
@Strain 300 %
ASTM Oil #3, 504; ASTM D471
 9.70 MPa
@Strain 300 %
1410 psi
@Strain 300 %
ASTM D412
 10.67 MPa
@Strain 300 %
1548 psi
@Strain 300 %
ASTM Oil #3, 336; ASTM D471
 10.961 MPa
@Strain 300 %
1589.8 psi
@Strain 300 %
ASTM Oil #3, 70; ASTM D471
 11.931 MPa
@Strain 300 %
1730.4 psi
@Strain 300 %
ASTM Oil #3, 168; ASTM D471
 4.40 MPa
@Strain 100 %,
Temperature 100 °C
638 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D471
 4.62 MPa
@Strain 100 %,
Temperature 125 °C
670 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 336; ASTM D573
 4.675 MPa
@Strain 100 %,
Temperature 100 °C
678.1 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D471
 4.675 MPa
@Strain 100 %,
Temperature 125 °C
678.1 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 504; ASTM D573
 4.95 MPa
@Strain 100 %,
Temperature 100 °C
718 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 4.95 MPa
@Strain 100 %,
Temperature 100 °C
718 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 5.225 MPa
@Strain 100 %,
Temperature 100 °C
757.8 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 5.555 MPa
@Strain 100 %,
Temperature 100 °C
805.7 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 5.61 MPa
@Strain 100 %,
Temperature 100 °C
814 psi
@Strain 100 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 5.665 MPa
@Strain 100 %,
Temperature 100 °C
821.6 psi
@Strain 100 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 5.72 MPa
@Strain 100 %,
Temperature 125 °C
830 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 70; ASTM D573
 5.72 MPa
@Strain 100 %,
Temperature 125 °C
830 psi
@Strain 100 %,
Temperature 257 °F
Hot Air, 168; ASTM D573
 8.924 MPa
@Strain 300 %,
Temperature 125 °C
1294 psi
@Strain 300 %,
Temperature 257 °F
Hot Air, 336; ASTM D573
 9.70 MPa
@Strain 300 %,
Temperature 100 °C
1410 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 70; ASTM D573
 10.379 MPa
@Strain 300 %,
Temperature 100 °C
1505.3 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 168; ASTM D573
 10.476 MPa
@Strain 300 %,
Temperature 100 °C
1519.4 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 336; ASTM D573
 10.476 MPa
@Strain 300 %,
Temperature 125 °C
1519.4 psi
@Strain 300 %,
Temperature 257 °F
Hot Air, 168; ASTM D573
 10.67 MPa
@Strain 300 %,
Temperature 125 °C
1548 psi
@Strain 300 %,
Temperature 257 °F
Hot Air, 504; ASTM D573
 11.058 MPa
@Strain 300 %,
Temperature 100 °C
1603.8 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 70; ASTM D471
 11.058 MPa
@Strain 300 %,
Temperature 100 °C
1603.8 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 168; ASTM D471
 11.155 MPa
@Strain 300 %,
Temperature 100 °C
1617.9 psi
@Strain 300 %,
Temperature 212 °F
Hot Air, 504; ASTM D573
 11.64 MPa
@Strain 300 %,
Temperature 125 °C
1688 psi
@Strain 300 %,
Temperature 257 °F
Hot Air, 70; ASTM D573
 11.931 MPa
@Strain 300 %,
Temperature 100 °C
1730.4 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 50; ASTM D471
 12.125 MPa
@Strain 300 %,
Temperature 100 °C
1758.6 psi
@Strain 300 %,
Temperature 212 °F
ASTM Oil #1, 336; ASTM D471
 4.235 MPa
@Strain 100 %,
Time 1.21e+6 sec
614.2 psi
@Strain 100 %,
Time 336 hour
Fuel C; ASTM D471
 4.675 MPa
@Strain 100 %,
Time 1.81e+6 sec
678.1 psi
@Strain 100 %,
Time 504 hour
Fuel C; ASTM D471
 4.785 MPa
@Strain 100 %,
Time 605000 sec
694.0 psi
@Strain 100 %,
Time 168 hour
Fuel C; ASTM D471
 5.225 MPa
@Time 252000 sec,
Strain 100 %
757.8 psi
@Time 70.0 hour,
Strain 100 %
Fuel C; ASTM D471
 5.28 MPa
@Strain 100 %,
Time 1.21e+6 sec
766 psi
@Strain 100 %,
Time 336 hour
Fuel A; ASTM D471
 5.50 MPa
@Strain 100 %,
Time 605000 sec
798 psi
@Strain 100 %,
Time 168 hour
Fuel A; ASTM D471
 5.885 MPa
@Strain 100 %,
Time 1.81e+6 sec
853.5 psi
@Strain 100 %,
Time 504 hour
Fuel A; ASTM D471
 6.215 MPa
@Time 252000 sec,
Strain 100 %
901.4 psi
@Time 70.0 hour,
Strain 100 %
Fuel A; ASTM D471
 11.155 MPa
@Time 252000 sec,
Strain 300 %
1617.9 psi
@Time 70.0 hour,
Strain 300 %
Fuel A; ASTM D471
 30.723 MPa
@Strain 300 %,
Time 1.21e+6 sec
4456.0 psi
@Strain 300 %,
Time 336 hour
Fuel C; ASTM D471
 33.915 MPa
@Strain 300 %,
Time 1.81e+6 sec
4919.0 psi
@Strain 300 %,
Time 504 hour
Fuel C; ASTM D471
 35.112 MPa
@Time 605000 sec,
Strain 300 %
5092.6 psi
@Time 168 hour,
Strain 300 %
Fuel C; ASTM D471
 35.91 MPa
@Time 252000 sec,
Strain 300 %
5208 psi
@Time 70.0 hour,
Strain 300 %
Fuel C; ASTM D471
 48.279 MPa
@Strain 300 %,
Time 1.21e+6 sec
7002.3 psi
@Strain 300 %,
Time 336 hour
Fuel A; ASTM D471
 52.269 MPa
@Strain 300 %,
Time 1.81e+6 sec
7581.0 psi
@Strain 300 %,
Time 504 hour
Fuel A; ASTM D471
Elongation at Break 590 %590 %ASTM D412
 507.4 %
@Time 252000 sec
507.4 %
@Time 70.0 hour
Fuel A; ASTM D471
 531 %
@Time 1.21e+6 sec
531 %
@Time 336 hour
Fuel C; ASTM D471
 548.7 %
@Time 252000 sec
548.7 %
@Time 70.0 hour
Fuel C; ASTM D471
 548.7 %
@Time 605000 sec
548.7 %
@Time 168 hour
Fuel C; ASTM D471
 572.3 %
@Time 1.81e+6 sec
572.3 %
@Time 504 hour
Fuel C; ASTM D471
 590 %
@Time 605000 sec
590 %
@Time 168 hour
Fuel A; ASTM D471
 607.7 %
@Time 1.21e+6 sec
607.7 %
@Time 336 hour
Fuel A; ASTM D471
 637.2 %
@Time 1.81e+6 sec
637.2 %
@Time 504 hour
Fuel A; ASTM D471
 601.8 %
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
601.8 %
@Treatment Temp. 257 °F,
Time 504 hour
Hot Air; ASTM D573
 631.3 %
@Treatment Temp. 100 °C,
Time 605000 sec
631.3 %
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #1; ASTM D471
 660.8 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
660.8 %
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #1; ASTM D471
 660.8 %
@Treatment Temp. 100 °C,
Time 252000 sec
660.8 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #1; ASTM D471
 672.6 %
@Treatment Temp. 100 °C,
Time 252000 sec
672.6 %
@Treatment Temp. 212 °F,
Time 70.0 hour
ASTM Oil #3; ASTM D471
 678.5 %
@Treatment Temp. 100 °C,
Time 605000 sec
678.5 %
@Treatment Temp. 212 °F,
Time 168 hour
ASTM Oil #3; ASTM D471
 684.4 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
684.4 %
@Treatment Temp. 212 °F,
Time 504 hour
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 100 °C,
Time 605000 sec
684.4 %
@Treatment Temp. 212 °F,
Time 168 hour
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 125 °C,
Time 605000 sec
684.4 %
@Treatment Temp. 257 °F,
Time 168 hour
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
684.4 %
@Treatment Temp. 257 °F,
Time 336 hour
Hot Air; ASTM D573
 690.3 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
690.3 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #1; ASTM D471
 696.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
696.2 %
@Treatment Temp. 212 °F,
Time 70.0 hour
Hot Air; ASTM D573
 702.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
702.1 %
@Treatment Temp. 257 °F,
Time 70.0 hour
Hot Air; ASTM D573
 719.8 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
719.8 %
@Treatment Temp. 212 °F,
Time 336 hour
ASTM Oil #3; ASTM D471
 731.6 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
731.6 %
@Treatment Temp. 212 °F,
Time 336 hour
Hot Air; ASTM D573
 761.1 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
761.1 %
@Treatment Temp. 212 °F,
Time 504 hour
ASTM Oil #3; ASTM D471
Flexural Modulus  0.0269 GPa
@Thickness 584 mm
3.90 ksi
@Thickness 23.0 in
ASTM D790
 0.0590 GPa
@Thickness -762 mm
8.56 ksi
@Thickness -30.0 in
ASTM D790
Compressive Strength 0.300 MPa43.5 psi2% Deflection; ASTM D 575
 1.00 MPa145 psi5% Deflection; ASTM D 575
 2.10 MPa305 psi10% Deflection; ASTM D 575
 3.10 MPa450 psi15% Deflection; ASTM D 575
 4.30 MPa624 psi20% Deflection; ASTM D 575
 5.50 MPa798 psi25% Deflection; ASTM D 575
 16.5 MPa2390 psi50% Deflection; ASTM D 575
Resilience 4545[%], Bayshore; ASTM D2632
Tear Strength 87.6 kN/m500 pliDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 30
@Load 1.00 kg
30
@Load 2.20 lb
[mg] Loss, H-18; ASTM D3489
Compression Set  16 %
@Temperature 23.0 °C,
Time 79200 sec
16 %
@Temperature 73.4 °F,
Time 22.0 hour
postcured; ASTM D395-B
 19 %
@Temperature 23.0 °C,
Time 79200 sec
19 %
@Temperature 73.4 °F,
Time 22.0 hour
as molded; ASTM D395-B
 40 %
@Temperature 70.0 °C,
Time 79200 sec
40 %
@Temperature 158 °F,
Time 22.0 hour
postcured; ASTM D395-B
 80 %
@Temperature 70.0 °C,
Time 79200 sec
80 %
@Temperature 158 °F,
Time 22.0 hour
as molded; ASTM D395-B
 
Thermal PropertiesMetricEnglishComments
Vicat Softening Point 80.0 °C176 °FRate A; ASTM D1525
Brittleness Temperature >= -55.6 °C>= -68.0 °FASTM D746
Glass Transition Temp, Tg -46.0 °C-50.8 °F
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 177 - 193 °C351 - 379 °F
Middle Barrel Temperature 182 - 199 °C360 - 390 °F
Front Barrel Temperature 182 - 204 °C360 - 399 °F
Nozzle Temperature 185 - 207 °C365 - 405 °F
Zone 1 182 - 199 °C360 - 390 °FExtrusion
Zone 2 182 - 204 °C360 - 399 °FExtrusion
Zone 3 182 - 210 °C360 - 410 °FExtrusion
Die Temperature 188 - 210 °C370 - 410 °FExtrusion
Melt Temperature 190 - 205 °C374 - 401 °FExtrusion
 193 - 210 °C379 - 410 °FInjection
Mold Temperature 16.0 - 43.0 °C60.8 - 109 °F
Injection Pressure 41.4 - 103 MPa6000 - 15000 psiInjection
Hold Pressure 27.6 - 55.2 MPa4000 - 8000 psiInjection
Back Pressure <= 5.52 MPa<= 800 psiInjection
Cushion 0.317 - 0.635 cm0.125 - 0.250 inInjection
 
Compliance PropertiesMetricEnglishComments
FDA YesYes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Covestro Texin® 985 Thermoplastic Polyurethanes (TPU)
Covestro Texin® 970 U Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Lubrizol Pellethane® 2363-90A Thermoplastic Polyurethane Elastomer

PCOVEST0983a / 238172

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.