MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Covestro Texin® 985 Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Categories: Polymer; Thermoplastic; Polyurethane, TP

Material Notes: Texin 985 resin is an aromatic polyether-based thermoplastic polyurethane with a Shore hardness of approximately 85A. It can be processed by injection molding, extrusion, or blow molding.

Properties / Applications: Texin 985 resin offers outstanding abrasion resistance, impact strength, toughness, and flexibility. It also exhibits excellent inherent resistance to salt water stress cracking, and hydrolysis. Texin 985 natural color resin complies with FDA food-contact regulations 21 CFR 177.1680 (Polyurethane Resins) and 177.2600 (Rubber Articles Intended for Repeated Use), subject to the limitations of these and any other applicable regulations. In addition, Texin 985 natural color resin is listed under NSF standard 61 for use in potable water applications. Typical applications include gaskets, hose, tubing, shoe inserts, connectors, belting, and miscellaneous molded articles.

Information provided by Covestro

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.12 g/ccASTM D792
Linear Mold Shrinkage, Flow 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0080 cm/cm
@Thickness 2.54 mm
ASTM D955
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 85ASTM D2240
 76
@Time 1.81e+6 sec
Fuel C; ASTM D471
 77
@Time 252000 sec
Fuel C; ASTM D471
 77
@Time 605000 sec
Fuel C; ASTM D471
 83
@Time 252000 sec
Fuel A; ASTM D471
 84
@Time 605000 sec
Fuel A; ASTM D471
 84
@Time 1.81e+6 sec
Fuel A; ASTM D471
 85
@Time 1.21e+6 sec
Fuel A; ASTM D471
 85
@Time 1.21e+6 sec
Fuel C; ASTM D471
 70
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
 71
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
 72
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 75
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 76
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 77
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 77
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 78
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 78
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 80
@Treatment Temp. 125 °C,
Time 252000 sec
Hot Air; ASTM D573
 80
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
 80
@Treatment Temp. 125 °C,
Time 605000 sec
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 81
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
Tensile Strength at Break 38.6 MPaASTM D412
 19.3 MPa
@Time 1.21e+6 sec
Fuel C; ASTM D471
 23.932 MPa
@Time 252000 sec
Fuel C; ASTM D471
 24.704 MPa
@Time 1.81e+6 sec
Fuel C; ASTM D471
 25.476 MPa
@Time 605000 sec
Fuel C; ASTM D471
 37.056 MPa
@Time 252000 sec
Fuel A; ASTM D471
 39.758 MPa
@Time 605000 sec
Fuel A; ASTM D471
 43.223 MPa
@Time 1.21e+6 sec
Fuel A; ASTM D471
 43.618 MPa
@Time 1.81e+6 sec
Fuel A; ASTM D471
 11.58 MPa
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 12.738 MPa
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 16.212 MPa
@Treatment Temp. 125 °C,
Time 605000 sec
Hot Air; ASTM D573
 21.616 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
 24.318 MPa
@Treatment Temp. 125 °C,
Time 252000 sec
Hot Air; ASTM D573
 27.02 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #1; ASTM D471
 27.792 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 29.336 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 29.722 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
 32.81 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 35.512 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 36.284 MPa
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 36.284 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 39.758 MPa
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 40.144 MPa
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
 41.302 MPa
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
Tensile Stress at Strain 4.40 MPa
@Strain 100 %
ASTM Oil #3, 70; ASTM D471
 4.40 MPa
@Strain 100 %
ASTM Oil #3, 504; ASTM D471
 4.62 MPa
@Strain 100 %
ASTM Oil #3, 336; ASTM D471
 4.80 MPa
@Strain 50 %
ASTM D412
 4.95 MPa
@Strain 100 %
ASTM Oil #3, 168; ASTM D471
 5.50 MPa
@Strain 100 %
ASTM D412
 9.312 MPa
@Strain 300 %
ASTM Oil #3, 504; ASTM D471
 9.70 MPa
@Strain 300 %
ASTM D412
 10.67 MPa
@Strain 300 %
ASTM Oil #3, 336; ASTM D471
 10.961 MPa
@Strain 300 %
ASTM Oil #3, 70; ASTM D471
 11.931 MPa
@Strain 300 %
ASTM Oil #3, 168; ASTM D471
 4.40 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 168; ASTM D471
 4.62 MPa
@Strain 100 %,
Temperature 125 °C
Hot Air, 336; ASTM D573
 4.675 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 70; ASTM D471
 4.675 MPa
@Strain 100 %,
Temperature 125 °C
Hot Air, 504; ASTM D573
 4.95 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 70; ASTM D573
 4.95 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 504; ASTM D573
 5.225 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 168; ASTM D573
 5.555 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 336; ASTM D471
 5.61 MPa
@Strain 100 %,
Temperature 100 °C
Hot Air, 336; ASTM D573
 5.665 MPa
@Strain 100 %,
Temperature 100 °C
ASTM Oil #1, 50; ASTM D471
 5.72 MPa
@Strain 100 %,
Temperature 125 °C
Hot Air, 70; ASTM D573
 5.72 MPa
@Strain 100 %,
Temperature 125 °C
Hot Air, 168; ASTM D573
 8.924 MPa
@Strain 300 %,
Temperature 125 °C
Hot Air, 336; ASTM D573
 9.70 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 70; ASTM D573
 10.379 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 168; ASTM D573
 10.476 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 336; ASTM D573
 10.476 MPa
@Strain 300 %,
Temperature 125 °C
Hot Air, 168; ASTM D573
 10.67 MPa
@Strain 300 %,
Temperature 125 °C
Hot Air, 504; ASTM D573
 11.058 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 70; ASTM D471
 11.058 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 168; ASTM D471
 11.155 MPa
@Strain 300 %,
Temperature 100 °C
Hot Air, 504; ASTM D573
 11.64 MPa
@Strain 300 %,
Temperature 125 °C
Hot Air, 70; ASTM D573
 11.931 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 50; ASTM D471
 12.125 MPa
@Strain 300 %,
Temperature 100 °C
ASTM Oil #1, 336; ASTM D471
 4.235 MPa
@Strain 100 %,
Time 1.21e+6 sec
Fuel C; ASTM D471
 4.675 MPa
@Strain 100 %,
Time 1.81e+6 sec
Fuel C; ASTM D471
 4.785 MPa
@Strain 100 %,
Time 605000 sec
Fuel C; ASTM D471
 5.225 MPa
@Time 252000 sec,
Strain 100 %
Fuel C; ASTM D471
 5.28 MPa
@Strain 100 %,
Time 1.21e+6 sec
Fuel A; ASTM D471
 5.50 MPa
@Strain 100 %,
Time 605000 sec
Fuel A; ASTM D471
 5.885 MPa
@Strain 100 %,
Time 1.81e+6 sec
Fuel A; ASTM D471
 6.215 MPa
@Time 252000 sec,
Strain 100 %
Fuel A; ASTM D471
 11.155 MPa
@Time 252000 sec,
Strain 300 %
Fuel A; ASTM D471
 30.723 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel C; ASTM D471
 33.915 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel C; ASTM D471
 35.112 MPa
@Time 605000 sec,
Strain 300 %
Fuel C; ASTM D471
 35.91 MPa
@Time 252000 sec,
Strain 300 %
Fuel C; ASTM D471
 48.279 MPa
@Strain 300 %,
Time 1.21e+6 sec
Fuel A; ASTM D471
 52.269 MPa
@Strain 300 %,
Time 1.81e+6 sec
Fuel A; ASTM D471
Elongation at Break 590 %ASTM D412
 507.4 %
@Time 252000 sec
Fuel A; ASTM D471
 531 %
@Time 1.21e+6 sec
Fuel C; ASTM D471
 548.7 %
@Time 252000 sec
Fuel C; ASTM D471
 548.7 %
@Time 605000 sec
Fuel C; ASTM D471
 572.3 %
@Time 1.81e+6 sec
Fuel C; ASTM D471
 590 %
@Time 605000 sec
Fuel A; ASTM D471
 607.7 %
@Time 1.21e+6 sec
Fuel A; ASTM D471
 637.2 %
@Time 1.81e+6 sec
Fuel A; ASTM D471
 601.8 %
@Treatment Temp. 125 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 631.3 %
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #1; ASTM D471
 660.8 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #1; ASTM D471
 660.8 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #1; ASTM D471
 672.6 %
@Treatment Temp. 100 °C,
Time 252000 sec
ASTM Oil #3; ASTM D471
 678.5 %
@Treatment Temp. 100 °C,
Time 605000 sec
ASTM Oil #3; ASTM D471
 684.4 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 100 °C,
Time 605000 sec
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 125 °C,
Time 605000 sec
Hot Air; ASTM D573
 684.4 %
@Treatment Temp. 125 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 690.3 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #1; ASTM D471
 696.2 %
@Treatment Temp. 100 °C,
Time 252000 sec
Hot Air; ASTM D573
 702.1 %
@Treatment Temp. 125 °C,
Time 252000 sec
Hot Air; ASTM D573
 719.8 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
ASTM Oil #3; ASTM D471
 731.6 %
@Treatment Temp. 100 °C,
Time 1.21e+6 sec
Hot Air; ASTM D573
 761.1 %
@Treatment Temp. 100 °C,
Time 1.81e+6 sec
ASTM Oil #3; ASTM D471
Flexural Modulus 26.9 MPa
@Thickness 584 mm
ASTM D790
 59.0 MPa
@Thickness -762 mm
ASTM D790
Compressive Strength 0.300 MPa2% Deflection; ASTM D 575
 1.00 MPa5% Deflection; ASTM D 575
 2.10 MPa10% Deflection; ASTM D 575
 3.10 MPa15% Deflection; ASTM D 575
 4.30 MPa20% Deflection; ASTM D 575
 5.50 MPa25% Deflection; ASTM D 575
 16.5 MPa50% Deflection; ASTM D 575
Resilience 45[%], Bayshore; ASTM D2632
Tear Strength 87.6 kN/mDie C; ASTM D624
Taber Abrasion, mg/1000 Cycles 30
@Load 1.00 kg
[mg] Loss, H-18; ASTM D3489
Compression Set 16 %
@Temperature 23.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 19 %
@Temperature 23.0 °C,
Time 79200 sec
as molded; ASTM D395-B
 40 %
@Temperature 70.0 °C,
Time 79200 sec
postcured; ASTM D395-B
 80 %
@Temperature 70.0 °C,
Time 79200 sec
as molded; ASTM D395-B
 
Thermal PropertiesOriginal ValueComments
Vicat Softening Point 80.0 °CRate A; ASTM D1525
Brittleness Temperature >= -68.0 °FASTM D746
Glass Transition Temp, Tg -46.0 °C
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 177 - 193 °C
Middle Barrel Temperature 182 - 199 °C
Front Barrel Temperature 182 - 204 °C
Nozzle Temperature 185 - 207 °C
Zone 1 182 - 199 °CExtrusion
Zone 2 182 - 204 °CExtrusion
Zone 3 182 - 210 °CExtrusion
Die Temperature 188 - 210 °CExtrusion
Melt Temperature 190 - 205 °CExtrusion
 193 - 210 °CInjection
Mold Temperature 16.0 - 43.0 °C
Injection Pressure 6000 - 15000 psiInjection
Hold Pressure 4000 - 8000 psiInjection
Back Pressure <= 800 psiInjection
Cushion 0.125 - 0.250 inInjection
 
Compliance PropertiesOriginal ValueComments
FDA Yes

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Covestro Texin® 985 Thermoplastic Polyurethanes (TPU)
Covestro Texin® 970 U Thermoplastic Polyurethanes (TPU) (Extended Aging Data)
Lubrizol Pellethane® 2363-90A Thermoplastic Polyurethane Elastomer

PCOVEST0983a / 238172

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.