MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

VICTREX™ PEEK 450GL30 30% Glass Fiber Reinforced
Categories: Polymer; Thermoplastic; Polyketone; Polyetheretherketone (PEEK); Polyetheretherketone, PEEK, Glass Fiber Filled

Material Notes: High performance thermoplastic material, 30% glass fibre reinforced PolyEtherEtherKetone (PEEK), semi crystalline, granules for injection molding and extrusion, standard flow, FDA food contact compliant, color natural/beige.

Typical Application Areas: Applications for higher strength in a static system. Low coefficient of thermal expansion. Chemically resistant to aggressive environments, suitable for sterilization for medical and food contact applications.

Information provided by Victrex.

Vendors: Victrex is a global leader in high-performance PEEK and PAEK polymers, transforming industries from aerospace to medical devices. For 40 years, our innovative polymer solutions help customers achieve new levels of performance, sustainability, and cost efficiency across applications that millions rely on daily from smartphones to aircraft components. As pioneers in polymer engineering, we're committed to delivering transformational solutions that address global materials challenges. Visit www.victrex.com, call (800) VICTREX /1-484-342-6001, or email victrexplc@victrex.com.

Ensinger TECAPEEK™ shapes are manufactured exclusively with Victrex™ PEEK polymer. The Ensinger process and Victrex resins ensure reliability, consistency, dimensional stability, and high temperature mechanical performance.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.51 g/cc0.0546 lb/in³Crystalline; ISO 1183
Water Absorption at Saturation  0.30 %
@Temperature 23.0 °C
0.30 %
@Temperature 73.4 °F
SO 62-1
 0.45 %
@Temperature 100 °C
0.45 %
@Temperature 212 °F
SO 62-1
Viscosity 550000 cP
@Temperature 400 °C
550000 cP
@Temperature 752 °F
ISO 11443
Linear Mold Shrinkage 0.0030 cm/cm0.0030 in/in385°C nozzle, 190°C tool; ISO 294-4
Linear Mold Shrinkage, Transverse 0.0090 cm/cm0.0090 in/in385°C nozzle, 190°C tool; ISO 294-4
Spiral Flow  8.50 cm
@Thickness 1.00 mm
3.35 in
@Thickness 0.0394 in
Melt Temp: 180°C, Melt Temp: 385°C
 41.0 cm
@Thickness 3.00 mm
16.1 in
@Thickness 0.118 in
Melt Temp: 180°C, Melt Temp: 385°C
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 87.587.5ISO 868
Tensile Strength at Break  35.0 MPa
@Temperature 275 °C
5080 psi
@Temperature 527 °F
ISO 527
 60.0 MPa
@Temperature 175 °C
8700 psi
@Temperature 347 °F
ISO 527
 115 MPa
@Temperature 125 °C
16700 psi
@Temperature 257 °F
ISO 527
 185 MPa
@Temperature 23.0 °C
26800 psi
@Temperature 73.4 °F
ISO 527
Elongation at Break 2.8 %2.8 %ISO 527
Tensile Modulus 11.5 GPa1670 ksiISO 527
Flexural Strength  50.0 MPa
@Temperature 275 °C
7250 psi
@Temperature 527 °F
ISO 178
 80.0 MPa
@Temperature 175 °C
11600 psi
@Temperature 347 °F
ISO 178
 190 MPa
@Temperature 125 °C
27600 psi
@Temperature 257 °F
ISO 178
 275 MPa
@Temperature 23.0 °C
39900 psi
@Temperature 73.4 °F
ISO 178
Flexural Modulus 11.0 GPa1600 ksiISO 178
Compressive Strength  55.0 MPa
@Temperature 200 °C
7980 psi
@Temperature 392 °F
ISO 604
 160 MPa
@Temperature 120 °C
23200 psi
@Temperature 248 °F
ISO 604
 250 MPa
@Temperature 23.0 °C
36300 psi
@Temperature 73.4 °F
ISO 604
Izod Impact, Notched (ISO) 12.0 kJ/m²5.71 ft-lb/in²ISO 180/A
Izod Impact, Unnotched (ISO) 65.0 kJ/m²30.9 ft-lb/in²ISO 180/U
Charpy Impact Unnotched 5.50 J/cm²26.2 ft-lb/in²ISO 179/1U
Charpy Impact, Notched 0.800 J/cm²3.81 ft-lb/in²ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+16 ohm-cm1.00e+16 ohm-cm
Dielectric Constant 3.2
@Frequency 1000 Hz
3.2
@Frequency 1000 Hz
Dielectric Strength 25.0 kV/mm
@Thickness 2.00 mm
635 kV/in
@Thickness 0.0787 in
IEC 60243-1
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 150 V150 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  18.0 µm/m-°C
@Temperature <=143 °C
10.0 µin/in-°F
@Temperature <=289 °F
Below Tg; ISO 11359
 18.0 µm/m-°C
@Temperature >=143 °C
10.0 µin/in-°F
@Temperature >=289 °F
Above Tg; ISO 11359
CTE, linear, Transverse to Flow  45.0 µm/m-°C
@Temperature <=143 °C
25.0 µin/in-°F
@Temperature <=289 °F
Below Tg; ISO 11359
 110 µm/m-°C
@Temperature >=143 °C
61.1 µin/in-°F
@Temperature >=289 °F
Above Tg; ISO 11359
Thermal Conductivity 0.300 W/m-K2.08 BTU-in/hr-ft²-°FAverage; ISO 22007-4
 0.350 W/m-K2.43 BTU-in/hr-ft²-°FAlong flow; ISO 22007-4
Melting Point 343 °C649 °FISO 11357
Deflection Temperature at 1.8 MPa (264 psi) 328 °C622 °FISO 75-f
Glass Transition Temp, Tg 143 °C289 °FOnset; ISO 11357
 150 °C302 °FMidpoint; ISO 11357
UL RTI, Electrical 240 °C464 °FUL 746B
UL RTI, Mechanical with Impact 220 °C428 °FUL 746B
UL RTI, Mechanical without Impact 240 °C464 °FUL 746B
Glow Wire Test 960 °C
@Thickness 2.00 mm
1760 °F
@Thickness 0.0787 in
IEC 60695-2-12
 
Processing PropertiesMetricEnglishComments
Processing Temperature <= 100 °C<= 212 °FHopper Temperature
Rear Barrel Temperature 360 °C680 °F
Middle Barrel Temperature 370 - 375 °C698 - 707 °F
Front Barrel Temperature 380 °C716 °F
Nozzle Temperature 385 °C725 °F
Mold Temperature 180 - 200 °C356 - 392 °F
Dry Time 3.00 - 5.00 hour
@Temperature 120 - 150 °C
3.00 - 5.00 hour
@Temperature 248 - 302 °F
 
Descriptive Properties
Gate>2 mm or 0.5 x part thickness
Runner>3.5mmmanifold
 >3mm Die/nozzle

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
VICTREX™ PEEK 450G™ General Purpose
VICTREX™ PEEK 150GL30 30% Glass Fiber Reinforced
VICTREX™ PEEK 90HMF40 Polyetheretherketone (PEEK), 40% Carbon Fiber Reinforced
VICTREX™ PEEK 450CA30 30% Carbon Fiber Reinforced
Celanese Zytel® 70G33HS1L NC010 PA66-GF33

PVICT4 / 71828

Elmet Technologies

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.