MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Huntsman IROGRAN® A 98 E 4066 Polyester-Based TPU-High Performance Grade
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyurethane TPE; Polyurethane, TP; Thermoplastic Polyurethane, Elastomer, Polyester Grade

Material Notes: Introduction: IROGRAN A 98 E 4066 is a thermoplastic polyester- polyurethane for injection molding applications. Additional characteristics of the product are very short cycle times and high dimensional stability.

Performance Features:

  • Short cycle times
  • High demolding stability
  • High production rates
  • High wear resistance
  • High hydrolysis resistance
Applications: For the production of technical parts, wheels and rollers, coupling halfs, sprocket wheels, buffers.

Information provided by Huntsman

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.22 g/cc0.0441 lb/in³ASTM D792
Linear Mold Shrinkage 0.0070 cm/cm0.0070 in/inASTM D995
Melt Index of Compound 15 g/10 min
@Load 21.6 kg,
Temperature 210 °C
15 g/10 min
@Load 47.6 lb,
Temperature 410 °F
cm3/10 min
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 9797ASTM D2240
Hardness, Shore D 5959ASTM D2240
Tensile Strength at Break 50.0 MPa7250 psiDIN 53504
Elongation at Break 530 %530 %DIN 53504
100% Modulus 14.0 MPa
@Strain 100 %
2030 psi
@Strain 100 %
DIN 53504
300% Modulus 25.0 MPa
@Strain 300 %
3630 psi
@Strain 300 %
DIN 53504
Rebound 30 %30 %Bayshore; ASTM D2632
Tear Strength 135 kN/m770 pliASTM D624
Abrasion 3030[mm3]; ISO 4649
Compression Set  30 %
@Temperature 23.0 °C,
Time 252000 sec
30 %
@Temperature 73.4 °F,
Time 70.0 hour
ASTM D395
 45 %
@Temperature 70.0 °C,
Time 86400 sec
45 %
@Temperature 158 °F,
Time 24.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Feed Temperature 25.0 - 40.0 °C77.0 - 104 °FExtrusion
Front Barrel Temperature 165 - 190 °C329 - 374 °FExtrusion
Nozzle Temperature 170 - 200 °C338 - 392 °FExtrusion
 180 - 200 °C356 - 392 °FInjection Molding
Adapter Temperature 175 - 195 °C347 - 383 °FExtrusion
Die Temperature 175 - 200 °C347 - 392 °FExtrusion
Melt Temperature 170 - 195 °C338 - 383 °FInjection Molding
 185 - 200 °C365 - 392 °F
Mold Temperature 20.0 - 70.0 °C68.0 - 158 °FInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Huntsman IROGRAN® A 98 E 4735 Polyester-Based TPU-Injection Extrusion Grade
Huntsman IROGRAN® A 85 E 4993 FCM Polyester-Based TPU-Injection Extrusion Grade
Covestro Desmopan® 1050D TPU
Barlog Plastics KEBAFLEX P D40.3 Polyester-Elastomer, Shore D40
Celanese Hytrel® 4056 TPC-ET

PHU9905 / 150365

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.