MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

AK Steel 2205 Duplex Stainless steel
Categories: Metal; Ferrous Metal; Stainless Steel

Material Notes: AK Steel 2205 provides a combination of high strength, excellent corrosion resistance and stress-corrosion cracking resistance as well as very good pitting resistance, and low thermal expansion. The alloy is useful in a variety of applications that include heat exchangers, piping, pressure vessels, tanks, fans, pulp and paper production equipment, oilfield equipment and press rolls.

Information provided by AK Steel

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.82 g/cc0.283 lb/in³Estimated by MatWeb
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell C 2222
Tensile Strength, Ultimate 750 MPa109000 psi
Tensile Strength, Yield 510 MPa
@Strain 0.2 %
74000 psi
@Strain 0.2 %
Elongation at Break 35 %35 %in 2 inches
Charpy Impact, Notched  84.4 J/cm²
@Thickness 1.50 mm,
Temperature -40.0 °C
402 ft-lb/in²
@Thickness 0.0591 in,
Temperature -40.0 °F
Longitudinal
 131 J/cm²
@Thickness 1.50 mm,
Temperature -40.0 °C
623 ft-lb/in²
@Thickness 0.0591 in,
Temperature -40.0 °F
Longitudinal
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.020 %0.020 %
Chromium, Cr 22 %22 %
Iron, Fe 68.71 %68.71 %As Remainder
Molybdenum, Mo 3.1 %3.1 %
Nickel, Ni 6.0 %6.0 %
Nitrogen, N 0.17 %0.17 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Carlson 2205 (UNS S31803) Duplex Stainless Steel
Carlson 2205 (UNS S32205) Duplex Stainless Steel
Outokumpu 2205 Duplex Stainless Steel
Sandvik SANMAC SAF 2205 Bar Steel
MetalTek MTEK 2205 Cast UNS J92205 Duplex Stainless Steel

NAKS115 / 14718

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.