MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Special Metals INCONEL® Alloy 617
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A nickel-chromium-cobalt-molybdenum alloy with an exceptional combination of metallurgical stability, strength, and oxidation resistance at high temperatures. Resistance to oxidation is enhanced by an aluminum addition. The alloy also resists a wide range of corrosive aqueous environments. Used in gas turbines for combustion cans, ducting, and transition liners; for petrochemical processing; for heat-treating equipment; and in nitric acid production. Standard product forms are round, forging stock, extruded section, plate, sheet, strip, pipe, tube, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: UNS N06617; ASME SB-166, Boiler Code Sections I, VIII; AMS 5887, AMS 5888, AMS 5889; ASTM B166
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.36 g/cc0.302 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate  570 MPa
@Temperature 650 °C
82700 psi
@Temperature 1200 °F
Solution Annealed prior to test
 710 MPa
@Temperature 23.0 °C
103000 psi
@Temperature 73.4 °F
Tensile Strength, Yield 340 MPa
@Strain 0.2 %
49300 psi
@Strain 0.2 %
Solution Annealed. Value at room temperature
 220 MPa
@Strain 0.2 %,
Temperature 650 °C
31900 psi
@Strain 0.2 %,
Temperature 1200 °F
Solution Annealed prior to test
Elongation at Break 62 %62 %Solution Annealed
 50 %
@Temperature 650 °C
50 %
@Temperature 1200 °F
Solution Annealed prior to test.
Rupture Strength  10.3 MPa
@Temperature 1090 °C,
Time 3.60e+6 sec
1500 psi
@Temperature 2000 °F,
Time 1000 hour
 18.6 MPa
@Temperature 1090 °C,
Time 360000 sec
2700 psi
@Temperature 2000 °F,
Time 100 hour
 24.8 MPa
@Temperature 982 °C,
Time 3.60e+6 sec
3600 psi
@Temperature 1800 °F,
Time 1000 hour
 41.4 MPa
@Temperature 982 °C,
Time 360000 sec
6000 psi
@Temperature 1800 °F,
Time 100 hour
 96.5 MPa
@Temperature 816 °C,
Time 3.60e+6 sec
14000 psi
@Temperature 1500 °F,
Time 1000 hour
 145 MPa
@Temperature 816 °C,
Time 360000 sec
21000 psi
@Temperature 1500 °F,
Time 100 hour
 324 MPa
@Temperature 649 °C,
Time 3.60e+6 sec
47000 psi
@Temperature 1200 °F,
Time 1000 hour
 414 MPa
@Temperature 649 °C,
Time 360000 sec
60000 psi
@Temperature 1200 °F,
Time 100 hour
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000122 ohm-cm0.000122 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 11.6 µm/m-°C
@Temperature 20.0 - 100 °C
6.44 µin/in-°F
@Temperature 68.0 - 212 °F
Specific Heat Capacity 0.419 J/g-°C0.100 BTU/lb-°F
Thermal Conductivity 13.6 W/m-K94.4 BTU-in/hr-ft²-°F
Melting Point 1330 - 1380 °C2430 - 2520 °F
Solidus 1330 °C2430 °F
Liquidus 1380 °C2520 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.80 - 1.5 %0.80 - 1.5 %
Boron, B <= 0.0060 %<= 0.0060 %
Carbon, C 0.050 - 0.15 %0.050 - 0.15 %
Chromium, Cr 20 - 24 %20 - 24 %
Cobalt, Co 10 - 15 %10 - 15 %
Copper, Cu <= 0.50 %<= 0.50 %
Iron, Fe <= 3.0 %<= 3.0 %
Manganese, Mn <= 1.0 %<= 1.0 %
Molybdenum, Mo 8.0 - 10 %8.0 - 10 %
Nickel, Ni >= 44.5 %>= 44.5 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.015 %<= 0.015 %
Titanium, Ti <= 0.60 %<= 0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Special Metals INCONEL® Alloy 625
Special Metals INCONEL® Alloy 600
Special Metals INCONEL® Alloy 601
Special Metals Inconel® 604 Nickel Alloy Composition Spec

NINC32 / 17401

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.