MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Special Metals INCONEL® Alloy 617
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: A nickel-chromium-cobalt-molybdenum alloy with an exceptional combination of metallurgical stability, strength, and oxidation resistance at high temperatures. Resistance to oxidation is enhanced by an aluminum addition. The alloy also resists a wide range of corrosive aqueous environments. Used in gas turbines for combustion cans, ducting, and transition liners; for petrochemical processing; for heat-treating equipment; and in nitric acid production. Standard product forms are round, forging stock, extruded section, plate, sheet, strip, pipe, tube, and wire.

Data provided by the manufacturer, Special Metals.

Key Words: UNS N06617; ASME SB-166, Boiler Code Sections I, VIII; AMS 5887, AMS 5888, AMS 5889; ASTM B166
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.36 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 570 MPa
@Temperature 650 °C
Solution Annealed prior to test
 710 MPa
@Temperature 23.0 °C
Tensile Strength, Yield 340 MPa
@Strain 0.2 %
Solution Annealed. Value at room temperature
 220 MPa
@Strain 0.2 %,
Temperature 650 °C
Solution Annealed prior to test
Elongation at Break 62 %Solution Annealed
 50 %
@Temperature 650 °C
Solution Annealed prior to test.
Rupture Strength 1500 psi
@Temperature 1090 °C,
Time 3.60e+6 sec
 2700 psi
@Temperature 1090 °C,
Time 360000 sec
 3600 psi
@Temperature 982 °C,
Time 3.60e+6 sec
 6000 psi
@Temperature 982 °C,
Time 360000 sec
 14000 psi
@Temperature 816 °C,
Time 3.60e+6 sec
 21000 psi
@Temperature 816 °C,
Time 360000 sec
 47000 psi
@Temperature 649 °C,
Time 3.60e+6 sec
 60000 psi
@Temperature 649 °C,
Time 360000 sec
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000122 ohm-cm
 
Thermal PropertiesOriginal ValueComments
CTE, linear 11.6 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.419 J/g-°C
Thermal Conductivity 13.6 W/m-K
Melting Point 1330 - 1380 °C
Solidus 1330 °C
Liquidus 1380 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.80 - 1.5 %
Boron, B <= 0.0060 %
Carbon, C 0.050 - 0.15 %
Chromium, Cr 20 - 24 %
Cobalt, Co 10 - 15 %
Copper, Cu <= 0.50 %
Iron, Fe <= 3.0 %
Manganese, Mn <= 1.0 %
Molybdenum, Mo 8.0 - 10 %
Nickel, Ni >= 44.5 %
Silicon, Si <= 1.0 %
Sulfur, S <= 0.015 %
Titanium, Ti <= 0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Special Metals INCONEL® Alloy 718
Special Metals INCONEL® Alloy 625
Special Metals INCONEL® Alloy 600
Special Metals INCONEL® Alloy 601
Special Metals Inconel® 604 Nickel Alloy Composition Spec

NINC32 / 17401

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.