MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

ExxonMobil PP7855E1 Polypropylene Homopolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP)

Material Notes: Product Description: A high crystallinity, medium impact strength copolymer resin with high melt flow rate and good processing attributes. It is designed for injection-molded automotive interior applications and large appliance parts.

Availability: North America

Features:

  • Balanced Stiffness/Toughness
  • Good Stiffness
  • Impact Modified
  • Nucleated
  • Slip
Uses:
  • Appliances
  • Automotive Exterior Parts
  • Automotive Interior Parts
Processing Method: Injection Molding

Information provided by ExxonMobil

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.900 g/cc0.0325 lb/in³ExxonMobil Method
Melt Flow 30 g/10 min
@Load 2.16 kg,
Temperature 230 °C
30 g/10 min
@Load 4.76 lb,
Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 22.4 MPa3250 psi2.0 in/min; ASTM D638
Elongation at Yield 5.0 %5.0 %2.0 in/min; ASTM D638
Flexural Modulus, 1% Secant 1100 MPa160000 psi0.05 in/min; ASTM D790A
 1260 MPa183000 psi0.5 in/min; ASTM D790B
Izod Impact, Notched 1.71 J/cm3.20 ft-lb/inASTM D256A
Gardner Impact 26.6 J
@Thickness 3.17 mm,
Temperature -28.9 °C
19.6 ft-lb
@Thickness 0.125 in,
Temperature -20.0 °F
Geometry GC; ASTM D5420
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 94.4 °C202 °FASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo MAGNUM™ 3325 MT Acrylonitrile Butadiene Styrene (ABS) Resin
BASF Ultraform® H 4320 Q600 POM
Mitsubishi Iupital® F20-54 Copolymer Acetal
Trinseo PULSE™ 2000 EZ PC/ABS Engineering Resin
Celanese Celcon® M140 POM, Unfilled

PEX99410 / 175646

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.