MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

CRP Technology Windform® LX 2.0 Polyamide Composite
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Nylon (Polyamide PA)

Material Notes: Processed by selective laser sintering (SLS). Windform® LX 2.0 has improved the already excellent performances of Windform® LX and this can be noticed from technical properties and sinterability point of view. Windform® LX 2.0 is a new polyamide based material reinforced with new generation glass fiber system. The properties of Windform® LX 2.0 make it particularly suited for functional applications and finished complex parts. Windform® LX 2.0 is a naturally black material and is characterized by improved Ultimate Tensile Strength, increased stiffness as well as a high level of resistance to temperature, while providing an attractive surface finish. Windform® LX 2.0 also underlines its advantage towards Windform® GF, PRO and PRO B, with an excellent rate between quality and price. Windform® LX 2.0 is perfect to create functional prototypes or finished parts that require reliability, good temperature resistance and a captivating matte black color.

Sample applications: There are several fields of application: covers, latching systems, air intake systems, connectors, applications for drivers cockpit (e.i. steering wheel-mounted paddle shifters), but also cooling/ducted fans, UAV structural components, sport functional prototypes, performing design parts and stiff pieces for packaging, and other applications in the naval and aerospace industries.

Information provided by CRP Technology.

Vendors:   About CRP Technology
CRP Technology (Modena, Italy) develops, manufactures and sells its proprietary high performance composite materials Windform® for professional 3D Printing. It is also distinguished by its know-how in Selective Laser Sintering technology. It offers part production for short- and low-run production, and prototyping services with Windform®. Its specific application fields including but are not limited to: automotive and motorsports, design, aerospace, UAVs, marine, entertainment, defense, and packaging.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.311 g/cc0.04736 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 59.9 MPa8690 psiUNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Elongation at Break 2.3 %2.3 %UNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Tensile Modulus 6.248 GPa906.2 ksiUNI EN ISO 527-1(97) and UNI EN ISO 527-2(97)
Flexural Strength 92.2 MPa13400 psiUNI EN ISO 14125: 2000
Flexural Modulus 4.86 GPa705 ksiUNI EN ISO 14125: 2000
Charpy Impact Unnotched 1.814 J/cm²8.633 ft-lb/in²ISO 179-1:2007
Charpy Impact, Notched 0.437 J/cm²2.08 ft-lb/in²ISO 179-1:2007
 
Thermal PropertiesMetricEnglishComments
CTE, linear  36.3 µm/m-°C
@Temperature 60.0 - 110 °C
20.2 µin/in-°F
@Temperature 140 - 230 °F
X direction
 118.4 µm/m-°C
@Temperature 60.0 - 110 °C
65.78 µin/in-°F
@Temperature 140 - 230 °F
Y direction
 194.2 µm/m-°C
@Temperature 60.0 - 110 °C
107.9 µin/in-°F
@Temperature 140 - 230 °F
Z direction
Melting Point 180.0 °C356.0 °FASTM D3418
Deflection Temperature at 1.8 MPa (264 psi) 175.7 °C348.3 °FASTM D648
Vicat Softening Point 177.8 °C352.0 °F10 N; ASTM D1525
 
Descriptive Properties
ColorBlack
Surface Finish1.5 Ra µmAfter Finishing
 7.5 Ra µmAfter SLS Process

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
CRP Technology Windform® XT 2.0 Polyamide-Carbon Fiber Composite
CRP Technology Windform® SP Polyamide-Carbon Fiber Composite for 3D Printing
CRP Technology Windform® PS Polystyrene for Selective Laser Sintering
CRP Technology Windform® GT Polyamide Glass Composite
DSM Somos® PerFORM Stereolithography Polymer, UV Postcure

PCRPT40 / 130418

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.