MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Hot Work Steel
Categories: Metal; Ferrous Metal; Tool Steel; Hot Work Steel

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Hot Work Steel". Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 6.45 - 8.67 g/cc0.233 - 0.313 lb/in³Average value: 7.80 g/cc Grade Count:77
Particle Size 6.70 - 12.0 µm6.70 - 12.0 µmAverage value: 9.27 µm Grade Count:4
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 160 - 594160 - 594Average value: 271 Grade Count:24
Hardness, Knoop 431 - 660431 - 660Average value: 575 Grade Count:5
Hardness, Rockwell C 26.0 - 66.026.0 - 66.0Average value: 49.3 Grade Count:56
Hardness, Vickers 400 - 1250400 - 1250Average value: 657 Grade Count:7
Tensile Strength, Ultimate 1010 - 2310 MPa146000 - 335000 psiAverage value: 1650 MPa Grade Count:37
Tensile Strength, Yield 800 - 1900 MPa116000 - 276000 psiAverage value: 1390 MPa Grade Count:34
Elongation at Break 5.00 - 15.5 %5.00 - 15.5 %Average value: 10.6 % Grade Count:17
Elongation at Yield 10.0 - 16.0 %10.0 - 16.0 %Average value: 12.9 % Grade Count:5
Reduction of Area 15.0 - 55.0 %15.0 - 55.0 %Average value: 41.8 % Grade Count:21
Modulus of Elasticity 203 - 228 GPa29400 - 33000 ksiAverage value: 210 GPa Grade Count:38
Bulk Modulus 160 GPa23200 ksiAverage value: 160 GPa Grade Count:4
Machinability 45.0 - 95.0 %45.0 - 95.0 %Average value: 70.0 % Grade Count:17
Shear Modulus 80.0 - 81.0 GPa11600 - 11700 ksiAverage value: 80.5 GPa Grade Count:4
Charpy Impact 2.71 - 55.0 J2.00 - 40.6 ft-lbAverage value: 23.3 J Grade Count:15
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000500 - 0.0000590 ohm-cm0.0000500 - 0.0000590 ohm-cmAverage value: 0.0000524 ohm-cm Grade Count:7
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.00 - 14.3 µm/m-°C3.89 - 7.93 µin/in-°FAverage value: 12.3 µm/m-°C Grade Count:35
Specific Heat Capacity 0.418 - 0.461 J/g-°C0.100 - 0.110 BTU/lb-°FAverage value: 0.457 J/g-°C Grade Count:14
Thermal Conductivity 14.4 - 42.0 W/m-K99.9 - 291 BTU-in/hr-ft²-°FAverage value: 28.7 W/m-K Grade Count:31
Transformation Temperature 785 - 913 °C1450 - 1680 °FAverage value: 850 °C Grade Count:7
 
Processing PropertiesMetricEnglishComments
Processing Temperature 540 - 1220 °C1000 - 2230 °FAverage value: 856 °C Grade Count:21
Annealing Temperature 399 - 900 °C750 - 1650 °FAverage value: 782 °C Grade Count:13
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.220 - 2.10 %0.220 - 2.10 %Average value: 0.446 % Grade Count:86
Chromium, Cr 0.350 - 12.8 %0.350 - 12.8 %Average value: 4.44 % Grade Count:86
Cobalt, Co 2.00 - 4.50 %2.00 - 4.50 %Average value: 3.50 % Grade Count:3
Copper, Cu 0.250 %0.250 %Average value: 0.250 % Grade Count:12
Iron, Fe 71.3 - 98.2 %71.3 - 98.2 %Average value: 89.6 % Grade Count:86
Manganese, Mn 0.150 - 1.50 %0.150 - 1.50 %Average value: 0.454 % Grade Count:66
Molybdenum, Mo 0.200 - 8.50 %0.200 - 8.50 %Average value: 1.94 % Grade Count:73
Nickel, Ni 0.250 - 1.70 %0.250 - 1.70 %Average value: 0.703 % Grade Count:18
Phosphorus, P 0.0300 %0.0300 %Average value: 0.0300 % Grade Count:16
Silicon, Si 0.150 - 2.25 %0.150 - 2.25 %Average value: 0.769 % Grade Count:75
Sulfur, S 0.00100 - 0.0300 %0.00100 - 0.0300 %Average value: 0.0178 % Grade Count:30
Tungsten, W 1.00 - 19.0 %1.00 - 19.0 %Average value: 7.55 % Grade Count:20
Vanadium, V 0.100 - 5.40 %0.100 - 5.40 %Average value: 0.890 % Grade Count:79

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Cold Work Steel
Aluminum 413.0-F Die Casting Alloy
Aluminum A380.1 Composition Spec
Overview of materials for Medium Carbon Steel
Overview of materials for Air-Hardening Steel

M01033 / 81721

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.