MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Carlson C 800H Nickel-Iron-Chromium Alloy
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: General Description

Carlson Alloy C 800 is a nickel-iron-chromium alloy, combining high strength with excellent resistance to oxidation and carburization at elevated temperatures. This alloy resists sulfur attack, internal oxidation, scaling and corrosion in a wide variety of industrial atmospheres.

The high chromium content of C 800 assures good resistance to oxidation, while the nickel content imparts a fair degree of resistance to stress corrosion cracking.

Carlson Alloy C 800H is essentially the same alloy as C 800 except the carbon content is restricted to the upper portion of the specified range. C 800H also receives a solution-anneal which produces a coarser grain structure. This assures higher creep and rupture strengths, enabling C 800H to be used in applications that require prolonged exposure at elevated temperatures and/or in corrosive environments.

Applications

  • Chemical Processing – heat exchangers for nitric acid production; calciners, dryers and recuperators in soda ash plants; process equipment in fiberglass and ore processing plants.
  • Petroleum and Petrochemical – tubing for hydrotreaters and effluent coolers; tubing, manifolds, pigtails and quench lines in hydrogen reformers; flare tips for incinerating waste gasses in refineries; reformer tubing, catalyst grid supports and converters for ammonia production; ethylene furnaces; tubing, bends and flanges for vinyl chloride production; steam superheaters for styrene production.
  • Power Generation – boiler superheaters and reheater tubes and shields; gas turbine combustion cans, transition liners and diffusers.
  • Thermal Processing – baskets and boxes, fixtures and radiant tubes for heat treat furnaces.
  • Steel Production – coke plat quench-car liners and process piping; steam methane reformers and recuperators for direct reduction of iron ore.

Information provided by Carlson

Key Words: UNS N08810
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.94 g/cc0.287 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break >= 448 MPa>= 65000 psi
Tensile Strength, Ultimate  378 MPa
@Temperature 649 °C
54800 psi
@Temperature 1200 °F
 465 MPa
@Temperature 427 °C
67500 psi
@Temperature 800 °F
Tensile Strength, Yield  93.1 MPa
@Temperature 649 °C
13500 psi
@Temperature 1200 °F
 130 MPa
@Temperature 427 °C
18800 psi
@Temperature 800 °F
 >= 172 MPa
@Strain 0.2 %
>= 25000 psi
@Strain 0.2 %
Elongation at Break >= 30 %>= 30 %
Rupture Strength  5.52 MPa
@Temperature 982 °C,
Time 3.60e+8 sec
801 psi
@Temperature 1800 °F,
Time 100000 hour
 6.89 MPa
@Temperature 982 °C,
Time 1.08e+8 sec
999 psi
@Temperature 1800 °F,
Time 30000 hour
 8.27 MPa
@Temperature 982 °C,
Time 3.60e+7 sec
1200 psi
@Temperature 1800 °F,
Time 10000 hour
 89.63 MPa
@Temperature 649 °C,
Time 3.60e+8 sec
13000 psi
@Temperature 1200 °F,
Time 100000 hour
 103.42 MPa
@Temperature 649 °C,
Time 1.08e+8 sec
15000 psi
@Temperature 1200 °F,
Time 30000 hour
 120.65 MPa
@Temperature 649 °C,
Time 1.08e+8 sec
17499 psi
@Temperature 1200 °F,
Time 30000 hour
Modulus of Elasticity 197 GPa28500 ksi
 132 GPa
@Temperature 871 °C
19200 ksi
@Temperature 1600 °F
 169.9 GPa
@Temperature 427 °C
24640 ksi
@Temperature 800 °F
 
Electrical PropertiesMetricEnglishComments
Magnetic Permeability 1.0141.014200 Oersted
Curie Temperature -115 °C-175 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear 18.4 µm/m-°C
@Temperature 21.1 - 871 °C
10.2 µin/in-°F
@Temperature 70.0 - 1600 °F
Melting Point 1357 - 1385 °C2475 - 2525 °F
Solidus 1357 °C2475 °F
Liquidus 1385 °C2525 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.15 - 0.60 %0.15 - 0.60 %
Carbon, C 0.050 - 0.10 %0.050 - 0.10 %
Chromium, Cr 19 - 23 %19 - 23 %
Copper, Cu <= 0.75 %<= 0.75 %
Iron, Fe >= 39.5 %>= 39.5 %
Manganese, Mn <= 1.5 %<= 1.5 %
Nickel, Ni 30 - 35 %30 - 35 %
Silicon, Si <= 1.0 %<= 1.0 %
Sulfur, S <= 0.015 %<= 0.015 %
Titanium, Ti 0.15 - 0.60 %0.15 - 0.60 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
ATI Allvac® Nickelvac® A-286 Specialty Steel, Heat Treatment: 982°C (1800°F) + Age
21Cr-32Ni-Ti-Al IRON BASED 21Cr-32Ni-Ti-Al ALLOY FOR HEAT EXCHANGER SEAMLESS TUBES (NCF 800H TB)
ATI Allegheny Ludlum AL 800H™ Nickel-Base Alloy, UNS N08810
Carlson C 800 Nickel-Iron-Chromium Alloy
Aluminum 1100-H12

NCARLSO22 / 15829

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.