MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Muntz metal, UNS C28000, O61 Temper rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Fair to excellent corrosion resistance. Excellent hot formability and forgeability for blanking, forming and bending, hot forging and pressing, hot heading and upsetting, shearing.

Applications: architectural, large nuts and bolts, brazing rod, condenser plates, heat exchanger and condenser tubing, hot forgings.

Test specimen: rod - 25mm diameter.

Key Words: CDA 280, CZ109, ISO CuZn40, CEN CW509L, yellow metal, 60/40 brass
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.39 g/cc0.303 lb/in³
Grain Size  10 µm
@Treatment Temp. 425 °C
10 µm
@Treatment Temp. 797 °F
extruded, cold drawn 30%, annealed 1h
 13 µm
@Treatment Temp. 500 °C
13 µm
@Treatment Temp. 932 °F
extruded, cold drawn 30%, annealed 1h
 27 µm
@Treatment Temp. 600 °C
27 µm
@Treatment Temp. 1110 °F
extruded, cold drawn 30%, annealed 1h
 43 µm
@Treatment Temp. 690 °C
43 µm
@Treatment Temp. 1270 °F
extruded, cold drawn 30%, annealed 1h
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell F 8080
Tensile Strength, Ultimate 370 MPa53700 psi
 550 MPa79800 psias drawn, extruded, cold drawn 30%, annealed 1h
 375 MPa
@Treatment Temp. 500 °C
54400 psi
@Treatment Temp. 932 °F
extruded, cold drawn 30%, annealed 1h
 375 MPa
@Treatment Temp. 600 °C
54400 psi
@Treatment Temp. 1110 °F
extruded, cold drawn 30%, annealed 1h
 380 MPa
@Treatment Temp. 700 °C
55100 psi
@Treatment Temp. 1290 °F
extruded, cold drawn 30%, annealed 1h
 450 MPa
@Treatment Temp. 400 °C
65300 psi
@Treatment Temp. 752 °F
extruded, cold drawn 30%, annealed 1h
 520 MPa
@Treatment Temp. 300 °C
75400 psi
@Treatment Temp. 572 °F
extruded, cold drawn 30%, annealed 1h
 545 MPa
@Treatment Temp. 200 °C
79000 psi
@Treatment Temp. 392 °F
extruded, cold drawn 30%, annealed 1h
 550 MPa
@Treatment Temp. 100 °C
79800 psi
@Treatment Temp. 212 °F
extruded, cold drawn 30%, annealed 1h
Tensile Strength, Yield 145 MPa21000 psi
 360 MPa
@Strain 0.5 %
52200 psi
@Strain 0.5 %
as drawn, extruded, cold drawn 30%, annealed 1h
 105 MPa
@Strain 0.5 %,
Treatment Temp. 700 °C
15200 psi
@Strain 0.5 %,
Treatment Temp. 1290 °F
extruded, cold drawn 30%, annealed 1h
 120 MPa
@Strain 0.5 %,
Treatment Temp. 600 °C
17400 psi
@Strain 0.5 %,
Treatment Temp. 1110 °F
extruded, cold drawn 30%, annealed 1h
 140 MPa
@Strain 0.5 %,
Treatment Temp. 500 °C
20300 psi
@Strain 0.5 %,
Treatment Temp. 932 °F
extruded, cold drawn 30%, annealed 1h
 190 MPa
@Strain 0.5 %,
Treatment Temp. 400 °C
27600 psi
@Strain 0.5 %,
Treatment Temp. 752 °F
extruded, cold drawn 30%, annealed 1h
 340 MPa
@Strain 0.5 %,
Treatment Temp. 300 °C
49300 psi
@Strain 0.5 %,
Treatment Temp. 572 °F
extruded, cold drawn 30%, annealed 1h
 370 MPa
@Strain 0.5 %,
Treatment Temp. 100 °C
53700 psi
@Strain 0.5 %,
Treatment Temp. 212 °F
extruded, cold drawn 30%, annealed 1h
 375 MPa
@Strain 0.5 %,
Treatment Temp. 200 °C
54400 psi
@Strain 0.5 %,
Treatment Temp. 392 °F
extruded, cold drawn 30%, annealed 1h
Elongation at Break 50 %50 %In 50 mm
 20 %
@Treatment Temp. 100 °C
20 %
@Treatment Temp. 212 °F
extruded, cold drawn 30%, annealed 1h
 21 %
@Treatment Temp. 200 °C
21 %
@Treatment Temp. 392 °F
extruded, cold drawn 30%, annealed 1h
 27 %
@Treatment Temp. 300 °C
27 %
@Treatment Temp. 572 °F
extruded, cold drawn 30%, annealed 1h
 47 %
@Treatment Temp. 400 °C
47 %
@Treatment Temp. 752 °F
extruded, cold drawn 30%, annealed 1h
 53 %
@Treatment Temp. 500 °C
53 %
@Treatment Temp. 932 °F
extruded, cold drawn 30%, annealed 1h
 53 %
@Treatment Temp. 600 °C
53 %
@Treatment Temp. 1110 °F
extruded, cold drawn 30%, annealed 1h
 53 %
@Treatment Temp. 700 °C
53 %
@Treatment Temp. 1290 °F
extruded, cold drawn 30%, annealed 1h
Tensile Modulus 103 GPa15000 ksi
 105 GPa15200 ksi
Poissons Ratio 0.350.35Calculated
Machinability 40 %40 %
Forgeability 90 %90 %
Shear Modulus 39.0 GPa5660 ksi
Shear Strength 275 MPa39900 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000610 ohm-cm0.00000610 ohm-cm28% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.8 µm/m-°C
@Temperature 20.0 - 300 °C
11.6 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.377 J/g-°C0.0900 BTU/lb-°F
Thermal Conductivity 123 W/m-K
@Temperature 20.0 °C
854 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 900 - 905 °C1650 - 1660 °F
Solidus 900 °C1650 °F
Liquidus 905 °C1660 °F
Annealing Point 427 - 593 °C800 - 1100 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 59 - 63 %59 - 63 %
Iron, Fe <= 0.070 %<= 0.070 %
Lead, Pb <= 0.30 %<= 0.30 %
Zinc, Zn 40 %40 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Muntz metal, UNS C28000, H01 Temper rod
Muntz metal, UNS C28000, M30 Temper rod
Muntz metal, UNS C28000, M20 Temper flat products
Muntz metal, UNS C28000, O61 Temper flat products
Mueller Ecostream™ GreenDrop™ C27450 Lead Free Plumbing Brass

MC28000b8 / 11157

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.