MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

Aluminum 518.0-F Die Casting Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes:

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 518.0-F; UNS A05180; AA518.0-F Die; Al518.0-F
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.57 g/cc0.0928 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 8080500 kg load, 10 mm ball
Hardness, Knoop 103103Estimated from Brinell Hardness.
Hardness, Rockwell B 4949Estimated from Brinell Hardness.
Hardness, Vickers 9090Estimated from Brinell Hardness.
Tensile Strength, Ultimate 310 MPa45000 psi
Tensile Strength, Yield 193 MPa
@Strain 0.2 %
28000 psi
@Strain 0.2 %
Elongation at Break 5.0 %5.0 %in 50 mm
Tensile Modulus 69.0 GPa10000 ksiEstimated
Poissons Ratio 0.330.33Estimated
Fatigue Strength 160 MPa
@# of Cycles 5.00e+8
23200 psi
@# of Cycles 5.00e+8
Notch Status unknown, R.R. Moore Test
Machinability 90 %90 %0-100 Scale (100=best)
Shear Modulus 26.0 GPa3770 ksiEstimated
Shear Strength 205 MPa29700 psi
Charpy Impact 9.00 J6.64 ft-lbV-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000680 ohm-cm0.00000680 ohm-cm
 
Thermal PropertiesMetricEnglishComments
Heat of Fusion 389 J/g167 BTU/lbTypical for cast aluminum
CTE, linear  24.1 µm/m-°C
@Temperature 20.0 °C
13.4 µin/in-°F
@Temperature 68.0 °F
 26.5 µm/m-°C
@Temperature 20.0 - 300 °C
14.7 µin/in-°F
@Temperature 68.0 - 572 °F
Estimated by MatWeb from similar alloys
Specific Heat Capacity 0.963 J/g-°C0.230 BTU/lb-°FTypical for cast aluminum
Thermal Conductivity 96.2 W/m-K668 BTU-in/hr-ft²-°F
Melting Point 535 - 621 °C995 - 1150 °F
Solidus 535 °C995 °F
Liquidus 621 °C1150 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 88.1 - 92.5 %88.1 - 92.5 %As remainder
Copper, Cu <= 0.25 %<= 0.25 %
Iron, Fe <= 1.8 %<= 1.8 %
Magnesium, Mg 7.5 - 8.5 %7.5 - 8.5 %
Manganese, Mn <= 0.35 %<= 0.35 %
Nickel, Ni <= 0.15 %<= 0.15 %
Other, total <= 0.25 %<= 0.25 %
Silicon, Si <= 0.35 %<= 0.35 %
Tin, Sn <= 0.15 %<= 0.15 %
Zinc, Zn <= 0.15 %<= 0.15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Aluminum LM4 TF (T6) Temper, Gravity Die Cast
Aluminum 390.0-T5 Conventional Die Cast
Aluminum B390.0-F Die Casting Alloy
Aluminum 390.0-F Conventional Die Cast
Aluminum A380.0-F Die Casting Alloy

MAC5180F / 10138

Free Trade Publications, Click Here!
Free Trade Publications, Click Here!

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.