MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay FM® 300M Epoxy Film Adhesive
Categories: Polymer; Adhesive; Thermoset; Epoxy; Epoxy Adhesive

Material Notes: Description: FM® 300 is a modified epoxy film adhesive available with three different moisture-resistant polyester carriers. It is designed for bonding metal-to-metal and sandwich composite structures. To achieve ultimate environmental resistance in bonding aluminum details, use pre-cured BR® 127 primer with FM 300 film adhesive. Extensively used as a surface finished ply on composites material outside layers, FM 300 film adhesive has unique properties which drastically reduce, and in some cases virtually eliminate, time-consuming sanding and filling operations. FM 300 film adhesive has high elongation and toughness with high ultimate shear strength. This makes it particularly suitable for redistributing the high shear stress concentrations of graphite epoxy- to-metal bonds, and allows it to accommodate the low interlaminar shear strength of the composite. It is particularly good in fatigue resistance in these joints. In properly designed and processed joints, the tight-knit tricot carrier provides a degree of electrical isolation between metal and graphite composites to reduce galvanic corrosion.

Features & Benefits:

  • Superior metal-to-metal peel strength, composite-to-composite bonding and composite-to-metal joints
  • Extensively used as surfacing ply for composite materials
  • Service temperature from -67°F to 300°F (-55°C to 150°C)
  • Excellent moisture and corrosion resistance in high humidity environments with no significant reduction in mechanical properties
  • Allows x-ray inspection of assemblies due to natural opacity of adhesive formulations
  • Available in a wide range of film thicknesses tailored to specific applications
  • Industry wide acceptance
Applications:
  • Metal-to-metal bonding
  • Composite-to-composite bonding
  • Composite-to-metal bonding
  • Composite surfacing

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Volatiles <= 1.0 %<= 1.0 %
Outgassing - Total Mass Loss 0.92 %0.92 %TWL
Collected Volatile Condensable Material 0.070 %0.070 %
Storage Temperature -18.0 °C-0.400 °FSupported Grades
 4.50 °C40.1 °FUnsupported Grades
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength 5.38 MPa780 psiFlatwise, 150°C for 7920 hrs
 6.55 MPa950 psiFlatwise, 150°C for 5760 hrs
 6.62 MPa960 psiFlatwise, 150°C for 2880 hrs
 6.83 MPa990 psiFlatwise, 150°C for 5040 hrs
 6.89 MPa1000 psiFlatwise, 150°C for 4320 hrs
 9.51 MPa1380 psiFlatwise, Heat Aging Control
 0.862 MPa
@Temperature 150 °C
125 psi
@Temperature 302 °F
Flatwise, 0.03 psf
 3.00 MPa
@Temperature 24.0 °C
435 psi
@Temperature 75.2 °F
Flatwise, 0.03 psf
 3.54 MPa
@Temperature 150 °C
513 psi
@Temperature 302 °F
Flatwise, 0.08 psf
 9.58 MPa
@Temperature 24.0 °C
1390 psi
@Temperature 75.2 °F
Flatwise, 0.08 psf
 11.0 MPa
@Temperature -55.0 °C
1600 psi
@Temperature -67.0 °F
Flatwise, 0.08 psf
Shear Strength 33.5 MPa4860 psi0.08 psf, after 200 hours in Skydrol4 hydraulic fluid at 150°F (66°C)
 35.34 MPa5125 psi0.08 psf, after 7 hays immersion in Hydrocarbon fluid
 36.2 MPa5250 psi0.08 psf, after 7 hays immersion in Anti-icing fluid
 36.9 MPa5350 psi0.08 psf, after 7 hays immersion in Hydraulic oil
 38.16 MPa5535 psi0.08 psf, after 30 days at 120°F (50°C), 95 – 100% RH3
 38.3 MPa5550 psi0.08 psf, after 7 hays immersion in JP-4 fuel
 15.9 MPa
@Temperature 150 °C
2310 psi
@Temperature 302 °F
0.03 psf
 17.9 - 20.0 MPa
@Temperature 150 °C
2600 - 2900 psi
@Temperature 302 °F
15 day Exposure at 54% RH
 20.37 MPa
@Temperature 150 °C
2955 psi
@Temperature 302 °F
0.08 psf
 20.4 MPa
@Temperature 149 °C
2960 psi
@Temperature 300 °F
150°C for 7920 hrs
 20.5 MPa
@Temperature 149 °C
2980 psi
@Temperature 300 °F
Heat Aging Control
 22.1 MPa
@Temperature 24.0 °C
3210 psi
@Temperature 75.2 °F
150°C for 5760 hrs
 22.5 MPa
@Temperature 24.0 °C
3270 psi
@Temperature 75.2 °F
150°C for 7920 hrs
 22.8 - 23.4 MPa
@Temperature 150 °C
3300 - 3400 psi
@Temperature 302 °F
no exposure
 23.2 MPa
@Temperature 120 °C
3360 psi
@Temperature 248 °F
0.03 psf
 23.4 MPa
@Temperature 149 °C
3400 psi
@Temperature 300 °F
150°C for 2880 hrs
 23.6 MPa
@Temperature 149 °C
3430 psi
@Temperature 300 °F
150°C for 4320 hrs
 23.8 MPa
@Temperature 149 °C
3450 psi
@Temperature 300 °F
150°C for 5760 hrs
 23.8 MPa
@Temperature 149 °C
3450 psi
@Temperature 300 °F
150°C for 7200 hrs
 24.3 MPa
@Temperature 149 °C
3530 psi
@Temperature 300 °F
150°C for 5040 hrs
 24.7 MPa
@Temperature 24.0 °C
3580 psi
@Temperature 75.2 °F
150°C for 7200 hrs
 25.6 MPa
@Temperature 149 °C
3720 psi
@Temperature 300 °F
150°C for 1140 hrs
 27.0 MPa
@Temperature 24.0 °C
3910 psi
@Temperature 75.2 °F
150°C for 5040 hrs
 27.9 MPa
@Temperature 120 °C
4040 psi
@Temperature 248 °F
0.08 psf
 29.6 MPa
@Temperature 24.0 °C
4300 psi
@Temperature 75.2 °F
150°C for 4320 hrs
 29.82 MPa
@Temperature 24.0 °C
4325 psi
@Temperature 75.2 °F
0.03 psf
 30.8 MPa
@Temperature 24.0 °C
4460 psi
@Temperature 75.2 °F
150°C for 1140 hrs
 32.4 MPa
@Temperature 24.0 °C
4700 psi
@Temperature 75.2 °F
150°C for 2880 hrs
 32.1 - 33.1 MPa
@Temperature 24.0 °C
4650 - 4800 psi
@Temperature 75.2 °F
no exposure
 34.0 MPa
@Temperature -55.0 °C
4930 psi
@Temperature -67.0 °F
0.08 psf
 33.8 - 35.9 MPa
@Temperature 24.0 °C
4900 - 5200 psi
@Temperature 75.2 °F
15 day Exposure at 54% RH
 36.37 MPa
@Temperature 24.0 °C
5275 psi
@Temperature 75.2 °F
0.08 psf
 41.9 MPa
@Temperature 24.0 °C
6070 psi
@Temperature 75.2 °F
Heat Aging Control
Peel Strength  4.03 kN/m
@Temperature 24.0 °C
23.0 pli
@Temperature 75.2 °F
Floating Roller, 0.03 psf
 4.56 kN/m
@Temperature 150 °C
26.0 pli
@Temperature 302 °F
Floating Roller, 0.08 psf
 4.73 kN/m
@Temperature 150 °C
27.0 pli
@Temperature 302 °F
Floating Roller, 0.03 psf
 4.91 - 5.08 kN/m
@Temperature 24.0 °C
28.0 - 29.0 pli
@Temperature 75.2 °F
Floating Roller, no exposure
 4.91 - 5.08 kN/m
@Temperature 24.0 °C
28.0 - 29.0 pli
@Temperature 75.2 °F
Floating Roller, 15 day Exposure at 54% RH
 5.08 kN/m
@Temperature 24.0 °C
29.0 pli
@Temperature 75.2 °F
Floating Roller, 0.08 psf
 5.08 kN/m
@Temperature -55.0 °C
29.0 pli
@Temperature -67.0 °F
Floating Roller, 0.08 psf
 11.9 - 13.1 kN/m
@Temperature 24.0 °C
68.0 - 75.0 pli
@Temperature 75.2 °F
Floating Roller, no exposure
 12.1 - 13.1 kN/m
@Temperature 150 °C
69.0 - 75.0 pli
@Temperature 302 °F
Floating Roller, 15 day Exposure at 54% RH
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 150 °C302 °F
Minimum Service Temperature, Air -55.0 °C-67.0 °F
 
Processing PropertiesMetricEnglishComments
Shelf Life 4.00 Month4.00 MonthUnsupported Grades
 12.0 Month12.0 MonthSupported Grades
 
Descriptive Properties
ColorGreen
Honeycomb Sandwich Peel16 Nm/mHoneycomb sandwich, 0.03 psf
 25 Nm/m150°C for 7920 hrs
 30 Nm/m150°C for 5760 hrs
 30 Nm/m150°C for 7200 hrs
 34 Nm/m150°C for 5040 hrs
 39 Nm/m150°C for 4320 hrs
 52 Nm/m150°C for 1140 hrs
 60 Nm/m150°C for 2880 hrs
 94 Nm/mHeat Aging Control

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay FM® 300 Epoxy Film Adhesive
300M Ultrahigh Strength Steel
Solvay FM® 73 Epoxy Film Adhesive
Henkel Hysol EA 9313 Paste Adhesive System
Latrobe Lescalloy® 300M - HS VAC-ARC High Strength Alloy Steel

PCYTED030 / 180332

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.