MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay BR® 6700-1 Bonding Primer
Categories: Polymer; Thermoset; Epoxy

Material Notes: Description: BR® 6700-1 corrosion inhibiting primer is a non-chromated, one-part, modified epoxy bonding primer which contains no volatile organic compounds (V.O.C.s). This primer is designed to meet stringent requirements of adhesive bonding primers on various metallic substrates and is compatible with PAA, PSA, PSA/TSA and Sol-Gel surface treatments. BR 6700-1 is 100% water based and does not rely on exempt solvents to achieve its zero V.O.C. level rating. It exceeds all state and federal V.O.C. emission regulations for structural adhesive bonding primers and offers mechanical properties and corrosion resistance equal to that of solvent-based primer systems. BR 6700-1 also provides outstanding performance with most 250°F to 350°F (121°C to 177°C) curing adhesive systems. BR 6700-1 has wide application/processing latitude, simple processing with H.V.L.P. or standard air atomizing spray equipment and is insensitive to spray booth conditions at temperatures from 65°F to 95°F (18°C to 35°C) and relative humidity from 30% to 70%.

Features & Benefits :

  • Zero V.O.C., 100% water-based
  • Non-chromated
  • Shows excellent film formation before curing
  • Scribe corrosion comparable to chromated primers and exceeds ASTM B117 specification
  • Short drying time, easy to determine when flash-off is complete
  • Drips and runs less likely to occur; clean up requires water only
  • Compatible with Sol-Gel surface treatment for titanium bonding and aluminum repair applications
  • Compatible with a wide variety of 250°F to 350°F (121°C to 177°C) curing adhesives
  • Mechanical properties comparable to solvent-based primer systems
  • Excellent performance at 0.00015 – 0.00035 inch (0.0038 – 0.0089 mm) primer thickness
  • Service temperature from -70°F to 350°F (-57°C to 177°C)
  • M.E.K. wipe resistant after 60 minute cure at 250°F (121°C)
  • Long storage life; 12 months at 40°F (4.4°C)
  • Coverage: 400 ft2/gal (9.8 m2/liter)

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³
Solids Content 25 %25 %
Storage Temperature 4.40 °C39.9 °F
 
Mechanical PropertiesMetricEnglishComments
Shear Strength 35.2 MPa5100 psiLap, 73M 121°C Cure Adhesive; ASTM D1002
 30.3 MPa
@Temperature 24.0 °C
4400 psi
@Temperature 75.2 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive, Pre-Test: 30 days at 49°C and 100% RH; ASTM D3165
 30.3 MPa
@Temperature 24.0 °C
4400 psi
@Temperature 75.2 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive, Pre-Test: 30 days Salt Fog exposure; ASTM D3165
 31.0 MPa
@Temperature -55.0 °C
4500 psi
@Temperature -67.0 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive; ASTM D3165
 32.1 MPa
@Temperature 24.0 °C
4650 psi
@Temperature 75.2 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive; ASTM D3165
 33.1 MPa
@Temperature 24.0 °C
4800 psi
@Temperature 75.2 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive, Pre-Test: 7 day soak in JP-4 at RT; ASTM D3165
 33.1 MPa
@Temperature 24.0 °C
4800 psi
@Temperature 75.2 °F
Wide Area Lap (Blister), 73M 121°C Cure Adhesive, Pre-Test: 7 day soak in hydraulic fluid at 66°C; ASTM D3165
Peel Strength 11.4 kN/m65.0 pliMetal-to-metal climbing drum, 73M 121°C Cure Adhesive
 11.4 kN/m65.0 pli
 10.5 kN/m
@Temperature -55.0 °C
60.0 pli
@Temperature -67.0 °F
Floating Roller, 73M 121°C Cure Adhesive; ASTM D3167
 12.3 kN/m
@Temperature 82.0 °C
70.0 pli
@Temperature 180 °F
Metal-to-metal climbing drum, 73M 121°C Cure Adhesive
 14.0 kN/m
@Temperature 24.0 °C
80.0 pli
@Temperature 75.2 °F
Floating Roller, 73M 121°C Cure Adhesive; ASTM D3167
 17.5 kN/m
@Temperature 24.0 °C
100 pli
@Temperature 75.2 °F
Metal-to-metal climbing drum, 73M 121°C Cure Adhesive
 17.5 kN/m
@Temperature 82.0 °C
100 pli
@Temperature 180 °F
Metal-to-metal climbing drum, 73M 121°C Cure Adhesive
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 177 °C351 °F
Minimum Service Temperature, Air -57.0 °C-70.6 °F
 
Processing PropertiesMetricEnglishComments
Shelf Life 12.0 Month12.0 Month
 
Descriptive Properties
ColorYellow

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay BR® 6747-1 Bonding Primer
Solvay BR® 6750 Water-Based Primer and Coating
Solvay FM® 385U Epoxy Film Adhesive
Dow Z-6701 SILANE
LKAB Minerals MicroCarb Chalk

PCYTED006 / 180308

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.