MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Solvay BR® 6747-1 Bonding Primer
Categories: Polymer; Thermoset; Epoxy

Material Notes: BR® 6747-1 corrosion inhibiting primer is a one part, chromate based, modified epoxy primer which contains no volatile organic components (VOC). BR 6747-1 is 100% water-based and does not rely on exempt solvents to achieve its zero VOC level rating. It exceeds all state and federal VOC emission regulations for structural adhesive bonding primers and offers mechanical properties and corrosion resistance equal to that of solvent-based primer systems. BR 6747-1 also provides outstanding performance with most 250 – 350°F (121 – 177°C) curing adhesive systems. BR 6747-1 offers wide application/processing latitude, simple processing with HVLP or standard air atomizing spray equipment and is insensitive to spray booth conditions at temperature from 65 – 95°F (18 – 35°C) and relative humidity from 30 – 70%.

Features & Benefits :

  • Zero V.O.C., 100% water-based
  • Short drying time, easy to determine when flash-off is complete
  • Drips and runs less likely to occur, clean-up requires water only
  • Spray gun clogging and tank scaling not an issue (rated at 600 hours continuous operation)
  • Excellent corrosion resistance
  • Can be cured from 250 – 350°F (121 – 177°C) and is compatible with a wide variety of 250 – 350°F (121 – 177°C) curing adhesives
  • Approved primer for AC-®130 bonding prep process (Boeing’s patented sol-gel technology)
  • Mechanical properties equal to solvent-based primer systems with primer thickness from 0.00015 to 0.0004 inches
  • Service temperature from -70°F to 350°F (-57°C to 177°C)
  • Protects prepared surface from further oxidation, prevents hydrolysis of oxide layers
  • MEK wipe resistant after 60 minute cure at 250°F (121°C)
  • Long storage life: 12 months at 40 – 50°F (4.5 – 12.8°C)
Suggested Applications:
  • Bond primer for aluminum components where corrosion protection is critical
  • Also very effective as a corrosion inhibiting paint primer for aluminium substrates.
  • Effective adhesion promoter for other metals (stainless steel, titanium, and nickel)
Note 1: Mechanical Properties with FM® 73, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 73, 0.060 lb/ft2 (293 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 2: Mechanical Properties with Metlbond 1146-3, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: Metlbond 1146M, 0.060 lb/ft2 (293 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 3: Mechanical Properties with Metlbond 1113, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: Metlbond 1113, 0.060 lb/ft2 (293 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 4: Mechanical Properties with FM® 123-2, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 123-2, 0.060 lb/ft2 (293 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 5: Mechanical Properties with FM® 87-1K, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 87-1K, 0.060 lb/ft2 (293 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 6: Mechanical Properties with FM® 300-2M, 250°F (121°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 300-2M, 0.085 lb/ft2 (415 gsm) adhesive cured 60 minutes at 250°F (121°C) under 40psi (275 kPa) pressure

Note 7: Mechanical Properties with Metlbond 1146, 350°F (177°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: Metlbond 1146M, 0.060 lb/ft2 (293 gsm) adhesive cured 90 minutes at 350°F (177°C) under 40psi (275 kPa) pressure

Note 8: Mechanical Properties with Metlbond 1515-3M, 350°F (177°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: Metlbond 1515-3M, 0.05 lb/ft2 (244 gsm) adhesive cured 90 minutes at 350°F (177°C) under 40psi (275 kPa) pressure

Note 9: Mechanical Properties with FM® 300, 350°F (177°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 300, 0.05 lb/ft2 (244 gsm) adhesive cured 90 minutes at 350°F (177°C) under 40psi (275 kPa) pressure

Note 10: Mechanical Properties with FM® 377S, 350°F (177°C) Cure Adhesive
Metal: 2024-T3 bare aluminum, surface treatment: FPL + PAA
Adhesive: FM 377S, 0.080 lb/ft2 (390 gsm) adhesive cured 90 minutes at 350°F (177°C) under 40psi (275 kPa) pressure

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.05 g/cc0.0379 lb/in³20% solid
 1.09 g/cc0.0394 lb/in³30% solid
Solids Content 20 %20 %
 30 %30 %
Volatile Organic Compounds (VOC) Content 0.00 g/l0.00 g/l
 
Mechanical PropertiesMetricEnglishComments
Shear Strength  11.7 MPa
@Temperature 177 °C
1700 psi
@Temperature 351 °F
Lap, Note 8
 11.7 MPa
@Temperature 177 °C
1700 psi
@Temperature 351 °F
Lap, Note 9
 12.4 MPa
@Temperature 149 °C
1800 psi
@Temperature 300 °F
Lap, Note 6
 14.8 MPa
@Temperature 177 °C
2150 psi
@Temperature 351 °F
Lap, Note 10
 23.4 MPa
@Temperature 121 °C
3400 psi
@Temperature 250 °F
Lap, Note 5
 23.4 MPa
@Temperature 82.0 °C
3400 psi
@Temperature 180 °F
Lap, Note 4
 23.8 MPa
@Temperature 121 °C
3450 psi
@Temperature 250 °F
Lap, Note 10
 24.1 MPa
@Temperature 121 °C
3500 psi
@Temperature 250 °F
Lap, Note 7
 24.8 MPa
@Temperature 177 °C
3600 psi
@Temperature 351 °F
Lap, Note 2
 26.2 MPa
@Temperature 82.0 °C
3800 psi
@Temperature 180 °F
Lap, Note 3
 28.7 MPa
@Temperature 24.0 °C
4160 psi
@Temperature 75.2 °F
Lap, Note 10
 29.6 MPa
@Temperature -55.0 °C
4300 psi
@Temperature -67.0 °F
Lap, Note 6
 31.0 MPa
@Temperature 82.0 °C
4500 psi
@Temperature 180 °F
Lap, Note 1
 31.7 MPa
@Temperature 24.0 °C
4600 psi
@Temperature 75.2 °F
Lap, Note 8
 31.7 MPa
@Temperature -55.0 °C
4600 psi
@Temperature -67.0 °F
Lap, Note 4
 31.7 MPa
@Temperature -55.0 °C
4600 psi
@Temperature -67.0 °F
Lap, Note 8
 34.5 MPa
@Temperature 24.0 °C
5000 psi
@Temperature 75.2 °F
Lap, Note 6
 35.2 MPa
@Temperature 24.0 °C
5100 psi
@Temperature 75.2 °F
Lap, Note 4
 37.9 MPa
@Temperature -55.0 °C
5500 psi
@Temperature -67.0 °F
Lap, Note 9
 38.6 MPa
@Temperature -55.0 °C
5600 psi
@Temperature -67.0 °F
Lap, Note 5
 41.4 MPa
@Temperature 24.0 °C
6000 psi
@Temperature 75.2 °F
Lap, Note 2
 41.4 MPa
@Temperature 24.0 °C
6000 psi
@Temperature 75.2 °F
Lap, Note 7
 41.4 MPa
@Temperature 24.0 °C
6000 psi
@Temperature 75.2 °F
Lap, Note 9
 42.7 MPa
@Temperature -55.0 °C
6200 psi
@Temperature -67.0 °F
Lap, Note 7
 44.8 MPa
@Temperature 24.0 °C
6500 psi
@Temperature 75.2 °F
Lap, Note 1
 44.8 MPa
@Temperature -55.0 °C
6500 psi
@Temperature -67.0 °F
Lap, Note 2
 45.5 MPa
@Temperature 24.0 °C
6600 psi
@Temperature 75.2 °F
Lap, Note 5
 46.9 MPa
@Temperature 24.0 °C
6800 psi
@Temperature 75.2 °F
Lap, Note 3
 48.3 MPa
@Temperature -55.0 °C
7000 psi
@Temperature -67.0 °F
Lap, Note 1
 50.3 MPa
@Temperature -55.0 °C
7300 psi
@Temperature -67.0 °F
Lap, Note 3
Peel Strength 4.21 kN/m24.0 pliMetal-to-Metal Climbing Drum, Note 10
 2.45 kN/m
@Temperature -55.0 °C
14.0 pli
@Temperature -67.0 °F
Floating Roller, Note 8
 2.45 kN/m
@Temperature -55.0 °C
14.0 pli
@Temperature -67.0 °F
Floating Roller, Note 9
 3.68 kN/m
@Temperature 24.0 °C
21.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 8
 4.21 kN/m
@Temperature 24.0 °C
24.0 pli
@Temperature 75.2 °F
Floating Roller, Note 8
 5.26 kN/m
@Temperature 24.0 °C
30.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 6
 5.61 kN/m
@Temperature 24.0 °C
32.0 pli
@Temperature 75.2 °F
Floating Roller, Note 6
 6.14 kN/m
@Temperature -55.0 °C
35.0 pli
@Temperature -67.0 °F
Floating Roller, Note 2
 6.14 kN/m
@Temperature -55.0 °C
35.0 pli
@Temperature -67.0 °F
Floating Roller, Note 7
 6.14 kN/m
@Temperature 24.0 °C
35.0 pli
@Temperature 75.2 °F
Floating Roller, Note 9
 6.14 kN/m
@Temperature 24.0 °C
35.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 9
 7.01 kN/m
@Temperature -55.0 °C
40.0 pli
@Temperature -67.0 °F
Floating Roller, Note 4
 7.36 kN/m
@Temperature -55.0 °C
42.0 pli
@Temperature -67.0 °F
Floating Roller, Note 5
 8.77 kN/m
@Temperature 107 °C
50.0 pli
@Temperature 225 °F
Floating Roller, Note 2
 9.64 kN/m
@Temperature -55.0 °C
55.0 pli
@Temperature -67.0 °F
Floating Roller, Note 3
 9.82 kN/m
@Temperature 107 °C
56.0 pli
@Temperature 225 °F
Floating Roller, Note 1
 9.99 kN/m
@Temperature 24.0 °C
57.0 pli
@Temperature 75.2 °F
Floating Roller, Note 4
 10.5 kN/m
@Temperature 24.0 °C
60.0 pli
@Temperature 75.2 °F
Floating Roller, Note 2
 10.5 kN/m
@Temperature 121 °C
60.0 pli
@Temperature 250 °F
Floating Roller, Note 7
 10.9 kN/m
@Temperature 24.0 °C
62.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 4
 10.9 kN/m
@Temperature -55.0 °C
62.0 pli
@Temperature -67.0 °F
Floating Roller, Note 1
 11.6 kN/m
@Temperature 24.0 °C
66.0 pli
@Temperature 75.2 °F
Floating Roller, Note 5
 12.3 kN/m
@Temperature 24.0 °C
70.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 3
 13.1 kN/m
@Temperature 24.0 °C
75.0 pli
@Temperature 75.2 °F
Floating Roller, Note 7
 14.4 kN/m
@Temperature 24.0 °C
82.0 pli
@Temperature 75.2 °F
Floating Roller, Note 1
 14.4 kN/m
@Temperature 24.0 °C
82.0 pli
@Temperature 75.2 °F
Floating Roller, Note 3
 15.4 kN/m
@Temperature 24.0 °C
88.0 pli
@Temperature 75.2 °F
Metal-to-Metal Climbing Drum, Note 5
 
Thermal PropertiesMetricEnglishComments
Maximum Service Temperature, Air 177 °C350 °F
Minimum Service Temperature, Air -56.7 °C-70.0 °F
 
Processing PropertiesMetricEnglishComments
Shelf Life  6.00 Month
@Temperature 14.0 - 24.0 °C
6.00 Month
@Temperature 57.2 - 75.2 °F
 12.0 Month
@Temperature 4.50 - 12.8 °C
12.0 Month
@Temperature 40.1 - 55.0 °F
 
Descriptive Properties
ColorYellow

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Solvay BR® 6700-1 Bonding Primer
Solvay BR® 6750 Water-Based Primer and Coating
Solvay BR® 154 Primer
Solvay FM® 385U Epoxy Film Adhesive
Solvay BR® 127 Primer with FM 73 Adhesive

PCYTED007 / 180309

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.