MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

EDRO #8 Premium 420 Stainless Mold Steel
Categories: Metal; Ferrous Metal; Stainless Steel; T 400 Series Stainless Steel

Material Notes: EDRO #8™ is a chromium-alloyed stainless tool steel with the following properties: excellent corrosion resistance, superior polishability, good wear resistance, good machinability, and stability in hardening.
EDRO #8™ is recommended for all types of molding tools, its special properties make it particularly suitable for molds with the following demands: corrosion/staining resistance, i.e., for molding of corrosive materials, e.g. PVC, acetates, and for molds subjected to humid working/storage conditions; Wear resistance, i.e., for molding abrasive/filled materials, including injection-molded thermosetting grades - also for molds with exceptionally long production runs, e.g. electrical/electronic parts; disposable cutlery and containers; High surface finish, i.e., for production of optical parts, such as camera and sunglass lenses, and for medical containers, e.g. syringes, analysis phials.
EDRO #8™ is resistant to corrosive attack by water, water vapor, weak organic acids, dilute solutions of nitrates, carbonates and other salts.

Information provided by EDRO

Key Words: AISI 420 improved, W.-Nr 1.2083
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density  7.67 g/cc
@Temperature 399 °C
0.277 lb/in³
@Temperature 750 °F
Hardened and tempered to 50 HRC
 7.75 g/cc
@Temperature 199 °C
0.280 lb/in³
@Temperature 390 °F
Hardened and tempered to 50 HRC
 7.81 g/cc
@Temperature 20.0 °C
0.282 lb/in³
@Temperature 68.0 °F
Hardened and tempered to 50 HRC
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 215215Delivery condition (soft annealed)
Hardness, Rockwell C  38
@Treatment Temp. 566 °C
38
@Treatment Temp. 1050 °F
Tempered twice for 2 hr at temperature
 50
@Treatment Temp. 482 °C
50
@Treatment Temp. 900 °F
Tempered twice for 2 hr at temperature
 52
@Treatment Temp. 177 °C
52
@Treatment Temp. 350 °F
Tempered twice for 2 hr at temperature
 53
@Treatment Temp. 260 °C
53
@Treatment Temp. 500 °F
Tempered twice for 2 hr at temperature
 55
@Treatment Temp. 399 °C
55
@Treatment Temp. 750 °F
Tempered twice for 2 hr at temperature
 55
@Treatment Temp. 93.3 °C
55
@Treatment Temp. 200 °F
Tempered twice for 2 hr at temperature
Tensile Strength, Ultimate 1420 MPa206000 psi45 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 1770 MPa256000 psi50 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 2070 MPa300000 psi55 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
Tensile Strength, Yield 1280 MPa185000 psi45 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 1470 MPa213000 psi50 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 1610 MPa234000 psi55 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
Elongation at Yield 8.0 %8.0 %in 2", 55 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 10 %10 %in 2", 50 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 12 %12 %in 2", 45 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
Reduction of Area 27 %27 %55 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 30 %30 %50 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
 40 %40 %45 HRC, Round bar 1" diameter, Hardened in oil from 1880°F and tempered twice
Modulus of Elasticity  190 GPa
@Temperature 399 °C
27500 ksi
@Temperature 750 °F
 210 GPa
@Temperature 199 °C
30400 ksi
@Temperature 390 °F
 214 GPa
@Temperature 20.0 °C
31100 ksi
@Temperature 68.0 °F
Izod Impact  16.3 J
@Treatment Temp. 510 °C
12.0 ft-lb
@Treatment Temp. 950 °F
Tempered for 2 hr
 20.3 J
@Treatment Temp. 371 °C
15.0 ft-lb
@Treatment Temp. 700 °F
Tempered for 2 hr
 20.3 J
@Treatment Temp. 149 °C
15.0 ft-lb
@Treatment Temp. 300 °F
Tempered for 2 hr
 27.1 J
@Treatment Temp. 260 °C
20.0 ft-lb
@Treatment Temp. 500 °F
Tempered for 2 hr
 32.5 J
@Treatment Temp. 649 °C
24.0 ft-lb
@Treatment Temp. 1200 °F
Tempered for 2 hr
 74.6 J
@Treatment Temp. 760 °C
55.0 ft-lb
@Treatment Temp. 1400 °F
Tempered for 2 hr
 
Thermal PropertiesMetricEnglishComments
CTE, linear  11.0 µm/m-°C
@Temperature 20.0 - 199 °C
6.10 µin/in-°F
@Temperature 68.0 - 390 °F
 11.5 µm/m-°C
@Temperature 20.0 - 399 °C
6.40 µin/in-°F
@Temperature 68.0 - 750 °F
Specific Heat Capacity 0.460 J/g-°C
@Temperature 20.0 °C
0.110 BTU/lb-°F
@Temperature 68.0 °F
Thermal Conductivity  22.9 W/m-K
@Temperature 20.0 °C
159 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
 23.9 W/m-K
@Temperature 199 °C
166 BTU-in/hr-ft²-°F
@Temperature 390 °F
 24.9 W/m-K
@Temperature 399 °C
173 BTU-in/hr-ft²-°F
@Temperature 750 °F
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.38 %0.38 %
Chromium, Cr 13.6 %13.6 %
Iron, Fe 84.42 %84.42 %As Balance
Manganese, Mn 0.50 %0.50 %
Silicon, Si 0.80 %0.80 %
Vanadium, V 0.30 %0.30 %
 
Descriptive Properties
Color CodeBrown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
420 Stainless Steel
304 Stainless Steel
Bohler-Uddeholm UDDEHOLM MIRRAX ESR Plastic Mold Steel
316 Stainless Steel, annealed strip
Kinetics MIM 420 Stainless Steel (Oil Quench Heat Treat)

NSEDRO008 / 142945

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.