MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Teknor Apex Medalist® MD-32265 Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Medalist MD-32265 is a high performance thermoplastic elastomer specifically designed for overmolding and multi-shot molding applications in the healthcare/medical segment. Medalist MD-32265 is a medium hardness, medium density, RoHS compliant grade that is sterilized, and is suitable for both injection and extrusion.

Availability: Africa & Middle East; Europe; Asia Pacific; Latin America; North America

Features: Bondability; BPA Free, Good Adhesion; Good Colorability; Good Compression Set; Good Flexibility; Good Impact Resistance; Good Moldability; Good Processability; Good Sterilizability; High Elasticity; Medium Hardness

Uses: Bonding; Flexible Grips; Gaskets; Handles; Jacketing; Medical Devices; Medical/Healthcare Applications; Overmolding; Pharmaceuticals; Rubber Replacement

Agency Ratings: ISO 10993 Part 5; ISO 13485

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding; Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.00 g/cc0.0361 lb/in³ASTM D792
Melt Flow 0.40 g/10 min
@Load 5.00 kg,
Temperature 200 °C
0.40 g/10 min
@Load 11.0 lb,
Temperature 392 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 6565ASTM D2240
Tensile Strength at Break 6.21 MPa900 psiASTM D412
Tensile Stress at Strain  2.14 MPa
@Strain 100 %
310 psi
@Strain 100 %
ASTM D412
 3.03 MPa
@Strain 200 %
440 psi
@Strain 200 %
ASTM D412
 4.00 MPa
@Strain 300 %
580 psi
@Strain 300 %
ASTM D412
Elongation at Break 600 %600 %ASTM D412
Tear Strength 30.7 kN/m175 pliASTM D624
Compression Set 20 %
@Temperature 22.8 °C,
Time 79200 sec
20 %
@Temperature 73.0 °F,
Time 22.0 hour
ASTM D395
 
Processing PropertiesMetricEnglishComments
Processing Temperature 282 - 302 °C540 - 575 °FMelt, Injection
Rear Barrel Temperature 193 - 216 °C380 - 420 °FInjection
Middle Barrel Temperature 260 - 282 °C500 - 540 °FInjection
Front Barrel Temperature 271 - 293 °C520 - 560 °FInjection
Nozzle Temperature 282 - 302 °C540 - 575 °FInjection
Zone 1 193 - 216 °C380 - 420 °FExtrusion
Zone 2 249 - 271 °C480 - 520 °FExtrusion
Zone 3 260 - 282 °C500 - 540 °FExtrusion
Zone 4 271 - 293 °C520 - 560 °FExtrusion
Die Temperature 271 - 293 °C520 - 560 °FExtrusion
Mold Temperature 21.1 - 37.8 °C70.0 - 100 °FInjection
Drying Temperature 60.0 °C140 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourInjection
Injection Pressure 1.38 - 5.52 MPa200 - 800 psiInjection
Back Pressure 0.172 - 0.689 MPa25.0 - 100 psiInjection
Cushion 0.381 - 2.54 cm0.150 - 1.00 inInjection
Screw Speed 30 - 100 rpm30 - 100 rpmExtrusion
 50 - 100 rpm50 - 100 rpmInjection
 
Descriptive Properties
AppearanceColors Available
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Teknor Apex Medalist® MD-17270 Thermoplastic Elastomer
Teknor Apex Medalist® MD-12362 Thermoplastic Elastomer
Teknor Apex Medalist® MD-34060 Thermoplastic Elastomer
Teknor Apex Medalist® MD-12160H Thermoplastic Elastomer
Teknor Apex Medalist® MD-50158 Thermoplastic Elastomer

PTEKNQ0721 / 237212

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.