MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

A. Schulman Diamond DIAMALOY GLY 7510 High Heat ASA Weatherable Polymer
Categories: Polymer; Thermoplastic; ASA Polymer; Acrylonitrile/Styrene/Acrylate (ASA), Unreinforced, Molded

Material Notes: Diamaloy GLY 7510 resin is a high gloss, high heat and high impact grade of ASA (acrylonitrile-styrene-acrylate) with good resistance to weather aging. This product is rated f1 by UL and be customed colored.

Applications:Typical applications include those requiring weatherability and toughness for automotive exterior applications and lawn and garden applications. As with any product, use of Diamaloy GLY 7510 resin in a given application must be tested (including but not limited to field testing) in advance by the user to determine suitability.

A. Schulman has acquired Network Polymers & Diamond Polymers.

Key Words: Weatherable Polymer
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.08 g/cc1.08 g/ccASTM D792
Linear Mold Shrinkage 0.0040 - 0.0070 cm/cm0.0040 - 0.0070 in/inASTM D955
Melt Flow  4.0 g/10 min
@Load 10.0 kg,
Temperature 220 °C
4.0 g/10 min
@Load 22.0 lb,
Temperature 428 °F
ASTM D1238
 8.3 g/10 min
@Load 5.00 kg,
Temperature 260 °C
8.3 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 101101ASTM D785
Tensile Strength at Break 38.0 MPa5510 psichs 2.0 in/min; ASTM D638
Tensile Strength, Yield 52.0 MPa7540 psichs 2.0 in/min; ASTM D638
Elongation at Break 22 %22 %chs 2.0 in/min; ASTM D638
Elongation at Yield 3.0 %3.0 %chs 2.0 in/min; ASTM D638
Tensile Modulus 2.784 GPa403.8 ksichs 2.0 in/min; ASTM D638
Flexural Strength 79.0 MPa
@Thickness 3.17 mm
11500 psi
@Thickness 0.125 in
chs 0.05 in/min; 2 in span; ASTM D790
Flexural Modulus 2.432 GPa
@Thickness 3.17 mm
352.7 ksi
@Thickness 0.125 in
chs 0.05 in/min; ASTM D790
Izod Impact, Notched  0.427 J/cm
@Thickness 3.17 mm,
Temperature -30.0 °C
0.800 ft-lb/in
@Thickness 0.125 in,
Temperature -22.0 °F
ASTM D256
 2.46 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
4.61 ft-lb/in
@Thickness 0.125 in,
Temperature 73.4 °F
ASTM D256
Instrumented Impact Total Energy  20.8 J
@Temperature -30.0 °C
15.3 ft-lb
@Temperature -22.0 °F
ASTM D3763
 27.0 J
@Temperature 23.0 °C
19.9 ft-lb
@Temperature 73.4 °F
ASTM D3763
 
Electrical PropertiesMetricEnglishComments
Hot Wire Ignition, HWI 3.0 sec3.0 secPLC Code; ASTM 746A
High Amp Arc Ignition, HAI 0.00 arcs0.00 arcsPLC Code; ASTM 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear 75.6 µm/m-°C
@Temperature -40.0 - 37.8 °C
42.0 µin/in-°F
@Temperature -40.0 - 100 °F
ASTM E831
CTE, linear, Transverse to Flow 86.4 µm/m-°C
@Temperature -40.0 - 37.8 °C
48.0 µin/in-°F
@Temperature -40.0 - 100 °F
ASTM E831
Deflection Temperature at 0.46 MPa (66 psi) 102 °C216 °F0.125";; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 88.0 °C190 °F0.125";; ASTM D648
Vicat Softening Point 104 °C219 °FASTM D1525
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
 
Optical PropertiesMetricEnglishComments
Gloss 94 %94 %Untextured; 60°; ASTM D523

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polycarbonate/ASA Alloy, Unreinforced
Trinseo Plexiglas® V825 Acrylic
INEOS Styrolution Luran® S KR 2859 ASA
SPS Guang Zhou POLOY™ 2001(+) PC/ABS
Polyram RamShine PAS701 ASA, UV Stabilized

PDIAM398 / 126489

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.