MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger SPI

Ensinger Tecatron® XP-61L Compression Molded PPS Compound, 25% Fiberglass and Mineral Filled
Categories: Polymer; Thermoplastic; Polyphenylene Sulfide (PPS); Polyphenylene Sulfide (PPS), Mineral/Glass-Fiber Filled

Material Notes: Ensinger Special Polymers has over twenty different grades of TECATRON PPS available. Custom formulations can be blended to suit specific applications. Compression molding is amenable to short run production and yields products which are homogenous with low process stress.

TECATRON PPS is a highly crystalline high-temperature thermoplastic with an excellent balance of cost, temperature resistance, strength, chemical resistance and flame retardance. TECATRON PPS is often used when long-term high-temperature performance and dimensional stability are a must, even in the presence of aggressive chemicals.

Applications:

  • Fuel Injectors
  • Manifolds
  • Pumps
  • Pistons
  • Gears
  • V-Packing Gaskets
  • Bearings

Information provided by Ensinger Special Polymers, Inc.

Vendors: Ensinger Special Polymers, Inc. provides consistent, high quality compression molded stock shapes of engineering thermoplastics. Common shapes include rings, rods, plates, tubes, and discs. Large diameter rings up to 90" OD are available.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.72 g/cc0.0621 lb/in³ASTM D792
Filler Content 25 %25 %
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 9797ASTM D785
Hardness, Shore D 9090ASTM D2240
Tensile Strength 42.1 MPa6100 psiASTM D638
Elongation at Break 1.0 %1.0 %ASTM D638
Tensile Modulus 8.96 GPa1300 ksiASTM D638
Flexural Strength 66.2 MPa9600 psiASTM D790
Flexural Modulus 6.89 GPa1000 ksiASTM D790
Compressive Strength 117 MPa17000 psiASTM D695
Shear Strength 55.2 MPa8000 psiASTM D732
Izod Impact, Notched 0.149 J/cm0.280 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
CTE, linear 57.6 µm/m-°C32.0 µin/in-°FASTM E831
Heat Distortion Temperature 251 °C484 °FASTM D648
 
Descriptive Properties
ColorDark Brown

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ensinger Tecatron® XP-64 Compression Molded PPS Compound, 40% Fiberglass
Celanese FORTRON 1342L4 PPS, 40% Specialty
Ensinger Tecatron® XP-65 Compression Molded PPS Compound, 30% Fiberglass with 15% PTFE
Ensinger Tecatron® XP-66 Compression Molded PPS Compound, 30% Fiberglass
Ensinger Tecatron® XP-81 Compression Molded PPS Compound, Filled with 15% Graphite and 15% Carbon Fiber

PENSIN941 / 140814

Master Bond adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.