MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Trinseo PULSE™ 920 MG PC/ABS
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate (PC)

Material Notes: An inherently matt medium heat, medium impact PC/ABS resin, PULSE™ 920 MG is designed for interior automotive applications where a matt aesthetic is required. Proprietary low gloss technology allows this unique combination of maximum low gloss aesthetics and physical properties.

Automotive Specifications:

  • DAIMLER DBL 5404.28
  • JLR STJLR.51.5229
  • JLR STJLR.51.353
  • JLR STJLR.51.5262
  • VOLKSWAGEN TL 522 31-A

Information provided by Dow

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Bulk Density 0.650 g/cc0.0235 lb/in³ISO 60
Density 1.12 g/cc0.0405 lb/in³ISO 1183/B
Volatile Organic Compounds (VOC) Content 9.0 g/l9.0 g/lVDA 277
Linear Mold Shrinkage 0.0035 - 0.0045 cm/cm0.0035 - 0.0045 in/inISO 294-4
Melt Flow  3.5 g/10 min
@Load 3.80 kg,
Temperature 230 °C
3.5 g/10 min
@Load 8.38 lb,
Temperature 446 °F
ISO 1133
 17 g/10 min
@Load 5.00 kg,
Temperature 260 °C
17 g/10 min
@Load 11.0 lb,
Temperature 500 °F
ISO 1133
Spiral Flow 51.0 cm20.1 inMelt Temp: 260°C, Injection Pressure 26100 psi
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 50.0 MPa7250 psi50mm/min; ISO 527
Elongation at Break 100 %100 %50mm/min; ISO 527
Tensile Modulus 2.25 GPa326 ksi1 mm/min; ISO 527
Flexural Modulus 2.10 GPa305 ksi2 mm/min; ISO 178
Charpy Impact, Notched  0.700 J/cm²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 2.20 J/cm²
@Temperature 23.0 °C
10.5 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Thermal PropertiesMetricEnglishComments
CTE, linear 73.0 µm/m-°C
@Temperature 0.000 - 80.0 °C
40.6 µin/in-°F
@Temperature 32.0 - 176 °F
ISO 11359-2
Deflection Temperature at 1.8 MPa (264 psi) 105 °C221 °Funannealed; ISO 75-A
Vicat Softening Point 122 °C252 °F50N / 50°C; ISO 306B
 
Processing PropertiesMetricEnglishComments
Melt Temperature 250 - 290 °C482 - 554 °F
Mold Temperature 70.0 - 90.0 °C158 - 194 °F
Drying Temperature 105 °C221 °F
Dry Time 4.00 hour4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Trinseo PULSE™ GX 70 PC/ABS Engineering Resin
Trinseo INSPIRE™ TF1500 ESU Polypropylene
Trinseo PULSE™ GX50 PC/ABS Engineering Resin
Zylog Hipolyene® X2 DP 4 Thermoplastic Polyolefin & PP Compound
Covestro Bayblend® KU 2-1473 Polycarbonate/ABS Blend

PZZDOW1161 / 30379

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.