MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Haynes 230® alloy, hot rolled and 1232°C solution annealed plate
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Excellent high-temperature strength, outstanding resistance to oxidizing environments up to 1149°C, premier resistance to nitriding environments, and excellent long-term thermal stability. Applications include combustion cans, transition ducts, flameholders, thermocouple sheaths and other gas turbine components; used for catalyst grid supports in ammonia burners, high-strength thermocouple protection tubes, high-temperature heat exchangers, ducts, high-temperature bellows; furnace retorts, chains and fixtures, burner flame shrouds, recuperator internals, dampers, nitriding furnace internals, heat-treating baskets, grates, trays, sparger tubes, and cyclone internals.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N06230, AMS 5878, AMS 5891, DIN 17742 No.2.4733
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 8.97 g/cc0.324 lb/in³at RT
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Ultimate 865 MPa125000 psi
 65.0 MPa
@Temperature 1204 °C
9430 psi
@Temperature 2199 °F
 91.0 MPa
@Temperature 1149 °C
13200 psi
@Temperature 2100 °F
 135 MPa
@Temperature 1093 °C
19600 psi
@Temperature 1999 °F
 245 MPa
@Temperature 982 °C
35500 psi
@Temperature 1800 °F
 435 MPa
@Temperature 871 °C
63100 psi
@Temperature 1600 °F
 605 MPa
@Temperature 760 °C
87700 psi
@Temperature 1400 °F
 675 MPa
@Temperature 649 °C
97900 psi
@Temperature 1200 °F
 705 MPa
@Temperature 538 °C
102000 psi
@Temperature 1000 °F
Tensile Strength, Yield 395 MPa
@Strain 0.2 %
57300 psi
@Strain 0.2 %
 30.0 MPa
@Strain 0.2 %,
Temperature 1204 °C
4350 psi
@Strain 0.2 %,
Temperature 2199 °F
 47.0 MPa
@Strain 0.2 %,
Temperature 1149 °C
6820 psi
@Strain 0.2 %,
Temperature 2100 °F
 75.0 MPa
@Strain 0.2 %,
Temperature 1093 °C
10900 psi
@Strain 0.2 %,
Temperature 1999 °F
 145 MPa
@Strain 0.2 %,
Temperature 982 °C
21000 psi
@Strain 0.2 %,
Temperature 1800 °F
 255 MPa
@Strain 0.2 %,
Temperature 871 °C
37000 psi
@Strain 0.2 %,
Temperature 1600 °F
 270 MPa
@Strain 0.2 %,
Temperature 649 °C
39200 psi
@Strain 0.2 %,
Temperature 1200 °F
 280 MPa
@Strain 0.2 %,
Temperature 538 °C
40600 psi
@Strain 0.2 %,
Temperature 1000 °F
 295 MPa
@Strain 0.2 %,
Temperature 760 °C
42800 psi
@Strain 0.2 %,
Temperature 1400 °F
Elongation at Break 49.6 %49.6 %in 50.8 mm
 52.5 %
@Temperature 760 °C
52.5 %
@Temperature 1400 °F
in 50.8 mm
 53 %
@Temperature 538 °C
53 %
@Temperature 1000 °F
in 50.8 mm
 55.3 %
@Temperature 649 °C
55.3 %
@Temperature 1200 °F
in 50.8 mm
 65.4 %
@Temperature 871 °C
65.4 %
@Temperature 1600 °F
in 50.8 mm
 82.7 %
@Temperature 1093 °C
82.7 %
@Temperature 1999 °F
in 50.8 mm
 83.1 %
@Temperature 982 °C
83.1 %
@Temperature 1800 °F
in 50.8 mm
 106.2 %
@Temperature 1149 °C
106.2 %
@Temperature 2100 °F
in 50.8 mm
 109.3 %
@Temperature 1204 °C
109.3 %
@Temperature 2199 °F
in 50.8 mm
Modulus of Elasticity 211 GPa30600 ksiRT
 150 GPa
@Temperature 1000 °C
21800 ksi
@Temperature 1830 °F
 157 GPa
@Temperature 900 °C
22800 ksi
@Temperature 1650 °F
 164 GPa
@Temperature 800 °C
23800 ksi
@Temperature 1470 °F
 171 GPa
@Temperature 700 °C
24800 ksi
@Temperature 1290 °F
 177 GPa
@Temperature 600 °C
25700 ksi
@Temperature 1110 °F
 184 GPa
@Temperature 500 °C
26700 ksi
@Temperature 932 °F
 190 GPa
@Temperature 400 °C
27600 ksi
@Temperature 752 °F
 196 GPa
@Temperature 300 °C
28400 ksi
@Temperature 572 °F
 202 GPa
@Temperature 200 °C
29300 ksi
@Temperature 392 °F
 207 GPa
@Temperature 100 °C
30000 ksi
@Temperature 212 °F
Charpy Impact 73.0 J53.8 ft-lbsolution annealed (unknown temp)
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000125 ohm-cm0.000125 ohm-cmRT
 0.000125 ohm-cm
@Temperature 1000 °C
0.000125 ohm-cm
@Temperature 1830 °F
 0.0001258 ohm-cm
@Temperature 100 °C
0.0001258 ohm-cm
@Temperature 212 °F
 0.0001265 ohm-cm
@Temperature 200 °C
0.0001265 ohm-cm
@Temperature 392 °F
 0.0001271 ohm-cm
@Temperature 900 °C
0.0001271 ohm-cm
@Temperature 1650 °F
 0.0001273 ohm-cm
@Temperature 300 °C
0.0001273 ohm-cm
@Temperature 572 °F
 0.0001284 ohm-cm
@Temperature 400 °C
0.0001284 ohm-cm
@Temperature 752 °F
 0.0001291 ohm-cm
@Temperature 800 °C
0.0001291 ohm-cm
@Temperature 1470 °F
 0.0001302 ohm-cm
@Temperature 500 °C
0.0001302 ohm-cm
@Temperature 932 °F
 0.0001307 ohm-cm
@Temperature 700 °C
0.0001307 ohm-cm
@Temperature 1290 °F
 0.0001312 ohm-cm
@Temperature 600 °C
0.0001312 ohm-cm
@Temperature 1110 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  12.7 µm/m-°C
@Temperature 25.0 - 100 °C
7.06 µin/in-°F
@Temperature 77.0 - 212 °F
 13.0 µm/m-°C
@Temperature 25.0 - 200 °C
7.22 µin/in-°F
@Temperature 77.0 - 392 °F
 13.3 µm/m-°C
@Temperature 25.0 - 300 °C
7.39 µin/in-°F
@Temperature 77.0 - 572 °F
 13.7 µm/m-°C
@Temperature 25.0 - 400 °C
7.61 µin/in-°F
@Temperature 77.0 - 752 °F
 14.0 µm/m-°C
@Temperature 25.0 - 500 °C
7.78 µin/in-°F
@Temperature 77.0 - 932 °F
 14.4 µm/m-°C
@Temperature 25.0 - 600 °C
8.00 µin/in-°F
@Temperature 77.0 - 1110 °F
 14.8 µm/m-°C
@Temperature 25.0 - 700 °C
8.22 µin/in-°F
@Temperature 77.0 - 1290 °F
 15.2 µm/m-°C
@Temperature 25.0 - 800 °C
8.44 µin/in-°F
@Temperature 77.0 - 1470 °F
 15.7 µm/m-°C
@Temperature 25.0 - 900 °C
8.72 µin/in-°F
@Temperature 77.0 - 1650 °F
 16.1 µm/m-°C
@Temperature 25.0 - 1000 °C
8.94 µin/in-°F
@Temperature 77.0 - 1830 °F
Specific Heat Capacity 0.397 J/g-°C0.0949 BTU/lb-°FRT
 0.419 J/g-°C
@Temperature 100 °C
0.100 BTU/lb-°F
@Temperature 212 °F
 0.435 J/g-°C
@Temperature 200 °C
0.104 BTU/lb-°F
@Temperature 392 °F
 0.448 J/g-°C
@Temperature 300 °C
0.107 BTU/lb-°F
@Temperature 572 °F
 0.465 J/g-°C
@Temperature 400 °C
0.111 BTU/lb-°F
@Temperature 752 °F
 0.473 J/g-°C
@Temperature 500 °C
0.113 BTU/lb-°F
@Temperature 932 °F
 0.486 J/g-°C
@Temperature 600 °C
0.116 BTU/lb-°F
@Temperature 1110 °F
 0.574 J/g-°C
@Temperature 700 °C
0.137 BTU/lb-°F
@Temperature 1290 °F
 0.595 J/g-°C
@Temperature 800 °C
0.142 BTU/lb-°F
@Temperature 1470 °F
 0.609 J/g-°C
@Temperature 900 °C
0.146 BTU/lb-°F
@Temperature 1650 °F
 0.617 J/g-°C
@Temperature 1000 °C
0.147 BTU/lb-°F
@Temperature 1830 °F
Thermal Conductivity 8.90 W/m-K61.8 BTU-in/hr-ft²-°FRT
 10.4 W/m-K
@Temperature 100 °C
72.2 BTU-in/hr-ft²-°F
@Temperature 212 °F
 12.4 W/m-K
@Temperature 200 °C
86.1 BTU-in/hr-ft²-°F
@Temperature 392 °F
 14.4 W/m-K
@Temperature 300 °C
99.9 BTU-in/hr-ft²-°F
@Temperature 572 °F
 16.4 W/m-K
@Temperature 400 °C
114 BTU-in/hr-ft²-°F
@Temperature 752 °F
 18.4 W/m-K
@Temperature 500 °C
128 BTU-in/hr-ft²-°F
@Temperature 932 °F
 20.4 W/m-K
@Temperature 600 °C
142 BTU-in/hr-ft²-°F
@Temperature 1110 °F
 22.4 W/m-K
@Temperature 700 °C
155 BTU-in/hr-ft²-°F
@Temperature 1290 °F
 24.4 W/m-K
@Temperature 800 °C
169 BTU-in/hr-ft²-°F
@Temperature 1470 °F
 26.4 W/m-K
@Temperature 900 °C
183 BTU-in/hr-ft²-°F
@Temperature 1650 °F
 28.4 W/m-K
@Temperature 1000 °C
197 BTU-in/hr-ft²-°F
@Temperature 1830 °F
Melting Point 1301 - 1371 °C2374 - 2500 °F
Solidus 1301 °C2374 °F
Liquidus 1371 °C2500 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 0.30 %0.30 %
Boron, B <= 0.015 %<= 0.015 %
Carbon, C 0.10 %0.10 %
Chromium, Cr 22 %22 %
Cobalt, Co <= 5.0 %<= 5.0 %
Iron, Fe <= 3.0 %<= 3.0 %
Lanthanum, La 0.020 %0.020 %
Manganese, Mn 0.50 %0.50 %
Molybdenum, Mo 2.0 %2.0 %
Nickel, Ni 57 %57 %
Silicon, Si 0.40 %0.40 %
Tungsten, W 14 %14 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Haynes 230® alloy plate
Haynes 214® Alloy Sheet
Haynes 188 alloy, 40% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 30% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 20% cold reduction, 3.2 mm thick sheet

NH23AJ / 16455

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.