MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes 230® alloy, hot rolled and 1232°C solution annealed plate
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Excellent high-temperature strength, outstanding resistance to oxidizing environments up to 1149°C, premier resistance to nitriding environments, and excellent long-term thermal stability. Applications include combustion cans, transition ducts, flameholders, thermocouple sheaths and other gas turbine components; used for catalyst grid supports in ammonia burners, high-strength thermocouple protection tubes, high-temperature heat exchangers, ducts, high-temperature bellows; furnace retorts, chains and fixtures, burner flame shrouds, recuperator internals, dampers, nitriding furnace internals, heat-treating baskets, grates, trays, sparger tubes, and cyclone internals.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N06230, AMS 5878, AMS 5891, DIN 17742 No.2.4733
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 8.97 g/ccat RT
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 865 MPa
 65.0 MPa
@Temperature 1204 °C
 91.0 MPa
@Temperature 1149 °C
 135 MPa
@Temperature 1093 °C
 245 MPa
@Temperature 982 °C
 435 MPa
@Temperature 871 °C
 605 MPa
@Temperature 760 °C
 675 MPa
@Temperature 649 °C
 705 MPa
@Temperature 538 °C
Tensile Strength, Yield 395 MPa
@Strain 0.2 %
 30.0 MPa
@Strain 0.2 %,
Temperature 1204 °C
 47.0 MPa
@Strain 0.2 %,
Temperature 1149 °C
 75.0 MPa
@Strain 0.2 %,
Temperature 1093 °C
 145 MPa
@Strain 0.2 %,
Temperature 982 °C
 255 MPa
@Strain 0.2 %,
Temperature 871 °C
 270 MPa
@Strain 0.2 %,
Temperature 649 °C
 280 MPa
@Strain 0.2 %,
Temperature 538 °C
 295 MPa
@Strain 0.2 %,
Temperature 760 °C
Elongation at Break 49.6 %in 50.8 mm
 52.5 %
@Temperature 760 °C
in 50.8 mm
 53 %
@Temperature 538 °C
in 50.8 mm
 55.3 %
@Temperature 649 °C
in 50.8 mm
 65.4 %
@Temperature 871 °C
in 50.8 mm
 82.7 %
@Temperature 1093 °C
in 50.8 mm
 83.1 %
@Temperature 982 °C
in 50.8 mm
 106.2 %
@Temperature 1149 °C
in 50.8 mm
 109.3 %
@Temperature 1204 °C
in 50.8 mm
Modulus of Elasticity 211 GPaRT
 150 GPa
@Temperature 1000 °C
 157 GPa
@Temperature 900 °C
 164 GPa
@Temperature 800 °C
 171 GPa
@Temperature 700 °C
 177 GPa
@Temperature 600 °C
 184 GPa
@Temperature 500 °C
 190 GPa
@Temperature 400 °C
 196 GPa
@Temperature 300 °C
 202 GPa
@Temperature 200 °C
 207 GPa
@Temperature 100 °C
Charpy Impact 73.0 Jsolution annealed (unknown temp)
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000125 ohm-cmRT
 0.000125 ohm-cm
@Temperature 1000 °C
 0.0001258 ohm-cm
@Temperature 100 °C
 0.0001265 ohm-cm
@Temperature 200 °C
 0.0001271 ohm-cm
@Temperature 900 °C
 0.0001273 ohm-cm
@Temperature 300 °C
 0.0001284 ohm-cm
@Temperature 400 °C
 0.0001291 ohm-cm
@Temperature 800 °C
 0.0001302 ohm-cm
@Temperature 500 °C
 0.0001307 ohm-cm
@Temperature 700 °C
 0.0001312 ohm-cm
@Temperature 600 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.7 µm/m-°C
@Temperature 25.0 - 100 °C
 13.0 µm/m-°C
@Temperature 25.0 - 200 °C
 13.3 µm/m-°C
@Temperature 25.0 - 300 °C
 13.7 µm/m-°C
@Temperature 25.0 - 400 °C
 14.0 µm/m-°C
@Temperature 25.0 - 500 °C
 14.4 µm/m-°C
@Temperature 25.0 - 600 °C
 14.8 µm/m-°C
@Temperature 25.0 - 700 °C
 15.2 µm/m-°C
@Temperature 25.0 - 800 °C
 15.7 µm/m-°C
@Temperature 25.0 - 900 °C
 16.1 µm/m-°C
@Temperature 25.0 - 1000 °C
Specific Heat Capacity 0.397 J/g-°CRT
 0.419 J/g-°C
@Temperature 100 °C
 0.435 J/g-°C
@Temperature 200 °C
 0.448 J/g-°C
@Temperature 300 °C
 0.465 J/g-°C
@Temperature 400 °C
 0.473 J/g-°C
@Temperature 500 °C
 0.486 J/g-°C
@Temperature 600 °C
 0.574 J/g-°C
@Temperature 700 °C
 0.595 J/g-°C
@Temperature 800 °C
 0.609 J/g-°C
@Temperature 900 °C
 0.617 J/g-°C
@Temperature 1000 °C
Thermal Conductivity 8.90 W/m-KRT
 10.4 W/m-K
@Temperature 100 °C
 12.4 W/m-K
@Temperature 200 °C
 14.4 W/m-K
@Temperature 300 °C
 16.4 W/m-K
@Temperature 400 °C
 18.4 W/m-K
@Temperature 500 °C
 20.4 W/m-K
@Temperature 600 °C
 22.4 W/m-K
@Temperature 700 °C
 24.4 W/m-K
@Temperature 800 °C
 26.4 W/m-K
@Temperature 900 °C
 28.4 W/m-K
@Temperature 1000 °C
Melting Point 1301 - 1371 °C
Solidus 1301 °C
Liquidus 1371 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 0.30 %
Boron, B <= 0.015 %
Carbon, C 0.10 %
Chromium, Cr 22 %
Cobalt, Co <= 5.0 %
Iron, Fe <= 3.0 %
Lanthanum, La 0.020 %
Manganese, Mn 0.50 %
Molybdenum, Mo 2.0 %
Nickel, Ni 57 %
Silicon, Si 0.40 %
Tungsten, W 14 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Haynes 230® alloy plate
Haynes 214® Alloy Sheet
Haynes 188 alloy, 40% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 30% cold reduction, 3.2 mm thick sheet
Haynes 188 alloy, 20% cold reduction, 3.2 mm thick sheet

NH23AJ / 16455

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.