MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Titanium Ti-5Al-2.5Sn, ELI, Annealed
Categories: Metal; Nonferrous Metal; Titanium Alloy; Alpha/Near Alpha Titanium Alloy

Material Notes: Annealed 700-870°C for 15 min-4 hr.

Characteristics: High service temperatures (480°C), Intermediate strength, Improved high temperature strength compared to unalloyed Ti, Excellent weld fabricability, Oxidation resistance, Microstructure stability, Nonheat-treatable (contains only iron impurity as a beta-stablizing element)

Applications: Gas turbine engine casings and rings, Aerospace structural members, Chemical processing equipment

Microstructure: Equiaxed alpha - when treated/worked below beta transus, Acicular alpha - when treated/worked above beta transus, Beta (bcc) - small amounts may be present

Forms typically available: Billet, bar, rod, plate, sheet, extrusions, and wire.

1 other heat treatment of this alloy is in MatWeb.

Key Words: UNS R54521 (ELI); Ti-5-2.5
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.48 g/cc0.162 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 311311Estimated from Rockwell C.
Hardness, Knoop 337337Estimated from Rockwell C.
Hardness, Rockwell C 3333
Hardness, Vickers 325325Estimated from Rockwell C.
Tensile Strength, Ultimate 775 MPa112000 psi
Tensile Strength, Yield 720 MPa104000 psi
Elongation at Break 18 %18 %
Creep Strength 276 MPa
@Temperature 204 °C,
Time >=3.60e+6 sec
40000 psi
@Temperature 399 °F,
Time >=1000 hour
strain 0.2%
Tensile Modulus 110 GPa16000 ksi
Notched Tensile Strength 1080 MPa157000 psiKt (stress concentration factor) = 6.3
Poissons Ratio 0.310.31Typical for alpha titanium alloy.
Fatigue Strength 410 MPa
@# of Cycles 1.00e+7
59500 psi
@# of Cycles 1.00e+7
Fracture Toughness 88.0 MPa-m½80.1 ksi-in½KIC
Shear Modulus 48.0 GPa6960 ksiStandard Ti-5-2.5
Charpy Impact 44.0 J32.5 ft-lbV-notch
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000160 ohm-cm0.000160 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.40 µm/m-°C
@Temperature 0.000 - 100 °C
5.22 µin/in-°F
@Temperature 32.0 - 212 °F
 9.50 µm/m-°C
@Temperature 0.000 - 315 °C
5.28 µin/in-°F
@Temperature 32.0 - 599 °F
average
Specific Heat Capacity  0.530 J/g-°C
@Temperature 20.0 °C
0.127 BTU/lb-°F
@Temperature 68.0 °F
 0.674 J/g-°C
@Temperature 315 °C
0.161 BTU/lb-°F
@Temperature 599 °F
Thermal Conductivity 7.80 W/m-K54.1 BTU-in/hr-ft²-°F
Melting Point <= 1590 °C<= 2890 °F
Liquidus 1590 °C2890 °F
Maximum Service Temperature, Air 480 °C896 °F
Beta Transus 1040 - 1090 °C1900 - 1990 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 5.0 %5.0 %
Iron, Fe <= 0.25 %<= 0.25 %
Oxygen, O <= 0.12 %<= 0.12 %
Tin, Sn 2.5 %2.5 %
Titanium, Ti 92.5 %92.5 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-5Al-2.5Sn (Grade 6)
European White Fir Wood
Titanium Ti-3Al-2.5V (Grade 9), Alpha-Beta Anneal, Quenched
Titanium Ti-6Al-2Nb-1Ta-0.8Mo (Ti-621/0.8), Alpha-Annealed
North American White Fir Wood

MTA521 / 14128

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.