MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 185,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Akro-Plastic Akromid® B3 GF 25 (2471) PA 6 Dry, 25% Glass Filled
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 30% Glass Fiber Filled

Material Notes: AKROMID® B (Polyamide 6) is an engineering compound, characterized by high mechanical strength, stiffness and thermal resistance. Furthermore, this polyamide offers high toughness at low temperatures as well as easy processing. AKROMID® B is an engineering plastic compound that allows a broad range of possible applications. On the basis of these standard types, we are able to develop individual compounds for special application needs.

Information from Akro-Plastic

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.31 g/cc
@Temperature 23.0 °C
0.0473 lb/in³
@Temperature 73.4 °F
ISO 1183
Filler Content 25 %25 %ISO 1172
Moisture Absorption 2.2 - 2.5 %
@Temperature 70.0 °C
2.2 - 2.5 %
@Temperature 158 °F
62% r.h., Humidity; ISO 62
Water Absorption at Saturation 6.8 - 7.4 %
@Time 82800 sec
6.8 - 7.4 %
@Time 23.0 hour
ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.0080 cm/cm0.0080 in/inISO 294-4
Spiral Flow 72.0 cm28.3 inCross Section: 7[mm]x3.5[mm]; AKRO
 
Mechanical PropertiesMetricEnglishComments
Ball Indentation Hardness 215 MPa31200 psiH 961/30; ISO 2039-1
Tensile Strength at Break 160 MPa23200 psi5 [mm/min]; ISO 527-1/2
 80.0 MPa
@Treatment Temp. 160 - 175 °C,
Time 1.80e+7 sec
11600 psi
@Treatment Temp. 320 - 347 °F,
Time 5000 hour
5 [mm/min], 50% Loss of Tensile Strength; ICE 216
 80.0 MPa
@Treatment Temp. 130 - 150 °C,
Time 7.20e+7 sec
11600 psi
@Treatment Temp. 266 - 302 °F,
Time 20000 hour
5 [mm/min], 50% Loss of Tensile Strength; ICE 216
Elongation at Break 3.5 %3.5 %5 [mm/min]; ISO 527-1/2
Tensile Modulus 8.50 GPa1230 ksi1[mm/min]; ISO 527-1/2
Flexural Strength 245 MPa35500 psi2 [mm/min]; ISO 178
Flexural Modulus 7.00 GPa1020 ksi2 [mm/min]; ISO 178
Charpy Impact Unnotched  8.00 J/cm²
@Temperature -30.0 °C
38.1 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eU
 8.50 J/cm²
@Temperature 23.0 °C
40.4 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  1.00 J/cm²
@Temperature -30.0 °C
4.76 ft-lb/in²
@Temperature -22.0 °F
ISO 179/1eA
 1.20 J/cm²
@Temperature 23.0 °C
5.71 ft-lb/in²
@Temperature 73.4 °F
ISO 179/1eA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+13 ohm-cm1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+12 ohm1.00e+12 ohmIEC 60093
Comparative Tracking Index 600 V600 VTest Solution A; IEC 60112
 
Thermal PropertiesMetricEnglishComments
Melting Point 220 °C428 °FISO 11357-1/3
Deflection Temperature at 0.46 MPa (66 psi) 220 °C428 °FHDT/B; ISO 75-2
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °FHDT/A; ISO 75-2
Flammability, UL94 HB
@Thickness 1.60 mm
HB
@Thickness 0.0630 in
Glow Wire Flammability Index 650 °C
@Thickness 1.60 mm
1200 °F
@Thickness 0.0630 in
ICE 60695-12
 
Processing PropertiesMetricEnglishComments
Feed Temperature 60.0 - 80.0 °C140 - 176 °F
Nozzle Temperature 240 - 280 °C464 - 536 °F
Zone 1 225 - 300 °C437 - 572 °F
Zone 2 225 - 300 °C437 - 572 °F
Zone 3 225 - 300 °C437 - 572 °F
Zone 4 225 - 300 °C437 - 572 °F
Melt Temperature 260 - 300 °C500 - 572 °F
Mold Temperature 80.0 - 100 °C176 - 212 °F
Drying Temperature 80.0 °C176 °F
Dry Time 2.00 hour2.00 hour
Hold Pressure 30.0 - 80.0 MPa4350 - 11600 psi
Back Pressure 5.00 - 10.0 MPa725 - 1450 psi
 
Descriptive Properties
Rate acc. FMVSS 302 (<100/min)Passed
Rate acc. FMVSS 302,(<100/min)FMVSS 302, >1 [mm] Thickness
Resistance to Oleic acidPass100% Conc. at 23°C
Resistance to AcetaldehydeFail40% Conc. at 23°C
Resistance to Acetic AcidPass20% Conc. at 23°C
Resistance to AcetonePass100% Conc. at 23°C
Resistance to AcetonitrilePass100% Conc. at 23°C
Resistance to AcrylonitrilePass100% Conc. at 23°C
Resistance to Allyl alcoholFail96% Conc. at 23°C
Resistance to Amyl alcoholPass100% Conc. at 23°C
Resistance to Aqueous AmmoniaPass10% Conc. at 23°C
Resistance to BenzeneFail100% Conc. at 40°C
 Pass100% Conc. at 23°C
 Pass100% Conc. at 23°C
Resistance to BiodieselPass100% Conc. at 23°C
Resistance to Boric acidFail100% Conc. at 23°C
 Pass10% Conc. at 23°C
Resistance to Brake fluid (DOT 4)Fail100% Conc. at 130°C
 Pass100% Conc. at 23°C
Resistance to Calcium chloride, alcoholicFail10% Conc. at 23°C
Resistance to Calcium chloride, aqueousPass10% Conc. at 23°C
Resistance to Carbonic acidPass100% Conc. at 60°C
Resistance to Caustic potash solution, aqueousPass50% Conc. at 23°C
Resistance to ChlorineFail100% Conc. at 23°C
Resistance to Chlorine waterFail100% Conc. at 23°C
Resistance to Chloroacetic acidFail50% Conc. at 23°C
Resistance to Chromic acidFail10% Conc. at 23°C
Resistance to CyclohexanePass100% Conc. at 23°C
Resistance to CyclohexanolPass100% Conc. at 23°C
Resistance to Dichloro-Acetic acidFail50% Conc. at 23°C
Resistance to Diesel fuel (DIN 51601)Pass100% Conc. at 23°C
Resistance to EthanolPass96% Conc. at 23°C
Resistance to Ethylene glycol/waterFail50% Conc. at 120°C
Resistance to Formaldehyde, aqueousPass10% Conc. at 23°C
Resistance to Formic acidFail2% Conc. at 23°C
Resistance to GlycerinPass100% Conc. at 23°C
Resistance to Hydraulic oil H and HL (DIN 51524)Pass100% Conc. at 100°C
Resistance to Hydrogen chloride, gasFail100% Conc. at 23°C
Resistance to Iso-octanolPass100% Conc. at 23°C
Resistance to IsopropanolPass100% Conc. at 23°C
Resistance to MethanolPass100% Conc. at 23°C
Resistance to Methylene chlorideFail100% Conc. at 23°C
Resistance to Motor oil (SAE 10W-40)Pass100% Conc. at 130°C
 Pass100% Conc. at 23°C
Resistance to Natural GasPass100% Conc. at 23°C
Resistance to Nitric acidFail40% Conc. at 23°C
Resistance to OzoneFail100% Conc. at 23°C
Resistance to PhenolFail100% Conc. at 23°C
Resistance to Phosphoric acidFail30% Conc. at 23°C
Resistance to Potassium chloride, aqueousPass10% Conc. at 23°C
Resistance to Potassium permanganate, aqueousFail10% Conc. at 23°C
Resistance to Sodium chloride, aqueousPass10% Conc. at 23°C
Resistance to Sodium hydroxide solution, aqueousPass1% Conc. at 23°C
Resistance to Sodium hypochlorite, aqueousFail10% Conc. at 23°C
Resistance to Transmission oil (ATF m 1375.4)Pass100% Conc. at 150°C
Resistance to Urea, aqueousPass20% Conc. at 23°C
Resistant to Carbon disulfidePass100% Conc. at 23°C
Resistant to Carbon tetrachloridePass100% Conc. at 23°C
Resistant to Citric acidPass10% Conc. at 23°C
Resistant to Ethyl acetatePass100% Conc. at 23°C
Resistant to Hydrochloric acidFail36% Conc. at 23°C
Resistant to Hydrogen peroxideFail23°C
Resistant to SeawaterPass100% Conc. at 23°C
Resistant to Silicone fluidPass23°C
Resistant to Sulfuric acidFail96% Conc. at 23°C
Resistant to Super-grade petrol (DIN 51600)Pass100% Conc. at 23°C
Resistant to ToluolPass100% Conc. at 23°C
Resistant to WaterPass100% Conc. up to 50°C
Resistant to XylolPass100% Conc. at 23°C
Resistant to Zinc chloride, aqueousFail50% Conc. at 23°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Akro-Plastic Akromid® B3 GF 50 (2475) PA 6 Dry, 50% Glass Filled
Akro-Plastic Akromid® B3 GF 10 (2829) PA 6 Dry, 10% Glass Filled
Akro-Plastic Akromid® A3 GF 30 4 L black (4678) PA 6 Dry, 30% Glass Filled
Akro-Plastic Akromid® A3 GF 25 (2420) PA 6.6 Dry, 25% Glass Filled
Azoty Tarnow™ Tarnamid® T-27 GF25 Polyamide 6 - Glass Fiber Reinforced

PAKRO029 / 126809

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.