Physical Properties | Metric | English | Comments |
---|
Density | 8.00 g/cc | 0.289 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 165 | 165 |
Tensile Strength, Ultimate | 570 MPa | 82700 psi |
| 380 MPa @Temperature 300 °C | 55100 psi @Temperature 572 °F |
| 390 MPa @Temperature 200 °C | 56600 psi @Temperature 392 °F |
| 430 MPa @Temperature 100 °C | 62400 psi @Temperature 212 °F |
| 840 MPa @Temperature -80.0 °C | 122000 psi @Temperature -112 °F |
| 1200 MPa @Temperature -196 °C | 174000 psi @Temperature -321 °F |
Tensile Strength, Yield | 220 MPa @Strain 0.2 % | 31900 psi @Strain 0.2 % |
| 280 MPa @Strain 0.2 % | 40600 psi @Strain 0.2 % |
| 320 MPa @Strain 1 % | 46400 psi @Strain 1 % |
| 110 MPa @Strain 0.2 %, Temperature 500 °C | 16000 psi @Strain 0.2 %, Temperature 932 °F |
| 115 MPa @Strain 0.2 %, Temperature 400 °C | 16700 psi @Strain 0.2 %, Temperature 752 °F |
| 127 MPa @Strain 0.2 %, Temperature 300 °C | 18400 psi @Strain 0.2 %, Temperature 572 °F |
| 139 MPa @Strain 1 %, Temperature 500 °C | 20200 psi @Strain 1 %, Temperature 932 °F |
| 144 MPa @Strain 1 %, Temperature 400 °C | 20900 psi @Strain 1 %, Temperature 752 °F |
| 147 MPa @Strain 0.2 %, Temperature 200 °C | 21300 psi @Strain 0.2 %, Temperature 392 °F |
| 156 MPa @Strain 1 %, Temperature 300 °C | 22600 psi @Strain 1 %, Temperature 572 °F |
| 177 MPa @Strain 0.2 %, Temperature 100 °C | 25700 psi @Strain 0.2 %, Temperature 212 °F |
| 177 MPa @Strain 1 %, Temperature 200 °C | 25700 psi @Strain 1 %, Temperature 392 °F |
| 211 MPa @Strain 1 %, Temperature 100 °C | 30600 psi @Strain 1 %, Temperature 212 °F |
| 275 MPa @Strain 0.2 %, Temperature -80.0 °C | 39900 psi @Strain 0.2 %, Temperature -112 °F |
| 350 MPa @Strain 0.2 %, Temperature -196 °C | 50800 psi @Strain 0.2 %, Temperature -321 °F |
| 355 MPa @Strain 1 %, Temperature -80.0 °C | 51500 psi @Strain 1 %, Temperature -112 °F |
| 450 MPa @Strain 1 %, Temperature -196 °C | 65300 psi @Strain 1 %, Temperature -321 °F |
Elongation at Break | 55 % | 55 % |
| 35 % @Temperature -196 °C | 35 % @Temperature -321 °F |
| 40 % @Temperature -80.0 °C | 40 % @Temperature -112 °F |
Modulus of Elasticity | 200 GPa | 29000 ksi |
| 165 GPa @Temperature 500 °C | 23900 ksi @Temperature 932 °F |
| 172 GPa @Temperature 400 °C | 24900 ksi @Temperature 752 °F |
| 179 GPa @Temperature 300 °C | 26000 ksi @Temperature 572 °F |
| 186 GPa @Temperature 200 °C | 27000 ksi @Temperature 392 °F |
| 194 GPa @Temperature 100 °C | 28100 ksi @Temperature 212 °F |
Poissons Ratio | 0.30 | 0.30 |
Fatigue Strength | 360 MPa @# of Cycles 2.00e+6 | 52200 psi @# of Cycles 2.00e+6 |
| 578 MPa @# of Cycles 2.00e+6 | 83800 psi @# of Cycles 2.00e+6 |
| 280 MPa @Strain 0.2 % | 40600 psi @Strain 0.2 % |
Shear Modulus | 77.0 GPa | 11200 ksi |
Impact Test | >= 60.0 J | >= 44.3 ft-lb |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.0000750 ohm-cm | 0.0000750 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 16.0 µm/m-°C @Temperature 100 °C | 8.89 µin/in-°F @Temperature 212 °F |
| 17.5 µm/m-°C @Temperature 400 °C | 9.72 µin/in-°F @Temperature 752 °F |
Specific Heat Capacity | 0.500 J/g-°C | 0.120 BTU/lb-°F |
Thermal Conductivity | 15.0 W/m-K | 104 BTU-in/hr-ft²-°F |
| 20.0 W/m-K @Temperature 400 °C | 139 BTU-in/hr-ft²-°F @Temperature 752 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.020 % | 0.020 % |
Chromium, Cr | 17.2 % | 17.2 % |
Iron, Fe | 70.58 % | 70.58 % |
Molybdenum, Mo | 2.1 % | 2.1 % |
Nickel, Ni | 10.1 % | 10.1 % |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.