MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C; Age 525°C (980°F)
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Excellent mechanical properties up to 315 °C. High strength and high toughness. Deep hardenability, excellent creep stability, excellent forgability.

Applications: Airframe applications, milling, forgings

Forms typically available: Billet, bar and plate

5 other heat treatments of this alloy are in MatWeb.

Key Words: KS 10-2-3 St 760ºC; Ti-10-2-3; TIMETAL 10-2-3
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 4.65 g/cc0.168 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Brinell 369369Estimated from Rockwell C.
Hardness, Knoop 403403Estimated from Rockwell C.
Hardness, Rockwell C 4040
Hardness, Vickers 450450
Tensile Strength, Ultimate 1240 MPa180000 psi
Tensile Strength, Yield 1200 MPa174000 psi(annealed 510°C)
Elongation at Break 6.0 %
@Thickness 15.0 mm
6.0 %
@Thickness 0.591 in
in 5 cm
Reduction of Area 10 %10 %
Tensile Modulus 106 GPa15400 ksi
Compressive Yield Strength 1160 MPa168000 psi
Compressive Modulus 110 GPa16000 ksi
Notched Tensile Strength 1480 MPa215000 psiKt (stress concentration factor) = 8.0
Ultimate Bearing Strength 2070 MPa300000 psie/D = 2
Bearing Yield Strength 1690 MPa245000 psie/D = 2
Poissons Ratio 0.330.33Typical for beta titanium alloy.
Fatigue Strength  450 MPa
@# of Cycles 1.00e+7
65300 psi
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 3.0
 700 MPa
@# of Cycles 10000
102000 psi
@# of Cycles 10000
Kt (stress concentration factor) = 3.0
 830 MPa
@# of Cycles 1.00e+7
120000 psi
@# of Cycles 1.00e+7
unnotched
 1000 MPa
@# of Cycles 1.00e+6
145000 psi
@# of Cycles 1.00e+6
unnotched
 1050 MPa
@# of Cycles 10000
152000 psi
@# of Cycles 10000
STA plate
Fracture Toughness 46.0 - 62.0 MPa-m½41.9 - 56.4 ksi-in½
Shear Modulus 41.0 GPa5950 ksi
Shear Strength 760 MPa110000 psiUltimate shear strength
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.000150 ohm-cm0.000150 ohm-cmEstimated from similar high-V-stabilized beta titanium alloys.
 
Thermal PropertiesMetricEnglishComments
CTE, linear  9.70 µm/m-°C
@Temperature 20.0 °C
5.39 µin/in-°F
@Temperature 68.0 °F
 9.70 µm/m-°C
@Temperature 20.0 - 425 °C
5.39 µin/in-°F
@Temperature 68.0 - 797 °F
average
Specific Heat Capacity 0.525 J/g-°C0.125 BTU/lb-°FTypical value for titanium alloys.
Thermal Conductivity 7.80 W/m-K54.1 BTU-in/hr-ft²-°FEstimated from similar high-V-stabilized beta titanium alloys.
Maximum Service Temperature, Air 315 °C599 °F
Beta Transus 760 °C1400 °F
 
Component Elements PropertiesMetricEnglishComments
Aluminum, Al 2.6 - 3.4 %2.6 - 3.4 %
Carbon, C <= 0.050 %<= 0.050 %
Hydrogen, H <= 0.015 %<= 0.015 %
Iron, Fe 1.6 - 2.2 %1.6 - 2.2 %
Nitrogen, N <= 0.050 %<= 0.050 %
Other, each <= 0.10 %<= 0.10 %
Other, total <= 0.30 %<= 0.30 %
Oxygen, O <= 0.13 %<= 0.13 %
Titanium, Ti 82.855 - 86.8 %82.855 - 86.8 %As Balance; Elemental Composition per ASTM B265
Vanadium, V 9.0 - 11 %9.0 - 11 %
 
Descriptive Properties
Crystal StructurebccBeta, predominant
 cphAlpha

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C, Aged 385°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) Solution Treated 850°C (1560°F)
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 730°C; overage 580°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 815°C, Anneal 620°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3), Anneal 1 hr. 760°C

MTB021 / 14145

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.