MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C; Age 525°C (980°F)
Categories: Metal; Nonferrous Metal; Titanium Alloy; Beta Titanium Alloy

Material Notes: Excellent mechanical properties up to 315 °C. High strength and high toughness. Deep hardenability, excellent creep stability, excellent forgability.

Applications: Airframe applications, milling, forgings

Forms typically available: Billet, bar and plate

5 other heat treatments of this alloy are in MatWeb.

Key Words: KS 10-2-3 St 760ºC; Ti-10-2-3; TIMETAL 10-2-3
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 4.65 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 369Estimated from Rockwell C.
Hardness, Knoop 403Estimated from Rockwell C.
Hardness, Rockwell C 40
Hardness, Vickers 450
Tensile Strength, Ultimate 1240 MPa
Tensile Strength, Yield 1200 MPa(annealed 510°C)
Elongation at Break 6.0 %
@Thickness 15.0 mm
in 5 cm
Reduction of Area 10 %
Tensile Modulus 106 GPa
Compressive Yield Strength 1160 MPa
Compressive Modulus 110 GPa
Notched Tensile Strength 1480 MPaKt (stress concentration factor) = 8.0
Ultimate Bearing Strength 2070 MPae/D = 2
Bearing Yield Strength 1690 MPae/D = 2
Poissons Ratio 0.33Typical for beta titanium alloy.
Fatigue Strength 450 MPa
@# of Cycles 1.00e+7
Kt (stress concentration factor) = 3.0
 700 MPa
@# of Cycles 10000
Kt (stress concentration factor) = 3.0
 830 MPa
@# of Cycles 1.00e+7
unnotched
 1000 MPa
@# of Cycles 1.00e+6
unnotched
 1050 MPa
@# of Cycles 10000
STA plate
Fracture Toughness 46.0 - 62.0 MPa-m½
Shear Modulus 41.0 GPa
Shear Strength 760 MPaUltimate shear strength
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000150 ohm-cmEstimated from similar high-V-stabilized beta titanium alloys.
 
Thermal PropertiesOriginal ValueComments
CTE, linear 9.70 µm/m-°C
@Temperature 20.0 °C
 9.70 µm/m-°C
@Temperature 20.0 - 425 °C
average
Specific Heat Capacity 0.525 J/g-°CTypical value for titanium alloys.
Thermal Conductivity 7.80 W/m-KEstimated from similar high-V-stabilized beta titanium alloys.
Maximum Service Temperature, Air 315 °C
Beta Transus 760 °C
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 2.6 - 3.4 %
Carbon, C <= 0.050 %
Hydrogen, H <= 0.015 %
Iron, Fe 1.6 - 2.2 %
Nitrogen, N <= 0.050 %
Other, each <= 0.10 %
Other, total <= 0.30 %
Oxygen, O <= 0.13 %
Titanium, Ti 82.855 - 86.8 %As Balance; Elemental Composition per ASTM B265
Vanadium, V 9.0 - 11 %
 
Descriptive Properties
Crystal StructurebccBeta, predominant
 cphAlpha

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 760°C, Aged 385°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) Solution Treated 850°C (1560°F)
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 730°C; overage 580°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3) ST 815°C, Anneal 620°C
Titanium Ti-10V-2Fe-3Al (Ti 10-2-3), Anneal 1 hr. 760°C

MTB021 / 14145

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.