MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polypropylene with 50% Glass Fiber Filler
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 50% Glass Fiber Filler

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene with 50% Glass Fiber Filler". Specific grades with glass content between 45% and 54% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.05 - 1.68 g/cc0.0379 - 0.0607 lb/in³Average value: 1.32 g/cc Grade Count:83
Filler Content 45.0 - 50.0 %45.0 - 50.0 %Average value: 49.1 % Grade Count:19
Water Absorption 0.0100 - 0.100 %0.0100 - 0.100 %Average value: 0.0589 % Grade Count:9
Linear Mold Shrinkage 0.000300 - 0.0350 cm/cm0.000300 - 0.0350 in/inAverage value: 0.00334 cm/cm Grade Count:30
 0.00300 - 0.00300 cm/cm
@Temperature 80.0 - 80.0 °C
0.00300 - 0.00300 in/in
@Temperature 176 - 176 °F
Average value: 0.00211 cm/cm Grade Count:1
 0.00200 - 0.00200 cm/cm
@Temperature 220 - 240 °C
0.00200 - 0.00200 in/in
@Temperature 428 - 464 °F
Average value: 0.00211 cm/cm Grade Count:4
 0.00200 - 0.00200 cm/cm
@Pressure 60.0 - 60.0 MPa
0.00200 - 0.00200 in/in
@Pressure 8700 - 8700 psi
Average value: 0.00211 cm/cm Grade Count:4
Linear Mold Shrinkage, Transverse 0.00400 - 0.0128 cm/cm0.00400 - 0.0128 in/inAverage value: 0.00858 cm/cm Grade Count:7
 0.00700 - 0.00700 cm/cm
@Temperature 80.0 - 80.0 °C
0.00700 - 0.00700 in/in
@Temperature 176 - 176 °F
Average value: 0.00700 cm/cm Grade Count:1
Melt Flow 1.20 - 15.0 g/10 min1.20 - 15.0 g/10 minAverage value: 5.30 g/10 min Grade Count:28
Ash 45.0 - 52.0 %45.0 - 52.0 %Average value: 48.3 % Grade Count:3
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 110 - 114110 - 114Average value: 112 Grade Count:4
Tensile Strength, Ultimate 47.0 - 400 MPa6820 - 58000 psiAverage value: 125 MPa Grade Count:66
 40.0 - 85.0 MPa
@Temperature 60.0 - 90.0 °C
5800 - 12300 psi
@Temperature 140 - 194 °F
Average value: 78.1 MPa Grade Count:12
Tensile Strength, Yield 5.60 - 142 MPa812 - 20600 psiAverage value: 108 MPa Grade Count:23
Elongation at Break 1.00 - 67.0 %1.00 - 67.0 %Average value: 3.27 % Grade Count:59
 2.20 - 5.80 %
@Temperature 60.0 - 90.0 °C
2.20 - 5.80 %
@Temperature 140 - 194 °F
Average value: 2.65 % Grade Count:12
Elongation at Yield 1.60 - 4.00 %1.60 - 4.00 %Average value: 2.34 % Grade Count:8
 2.70 - 4.20 %
@Temperature 60.0 - 90.0 °C
2.70 - 4.20 %
@Temperature 140 - 194 °F
Average value: 3.45 % Grade Count:1
Modulus of Elasticity 5.80 - 20.5 GPa841 - 2970 ksiAverage value: 11.3 GPa Grade Count:58
 5.30 - 8.40 GPa
@Temperature 60.0 - 90.0 °C
769 - 1220 ksi
@Temperature 140 - 194 °F
Average value: 7.70 GPa Grade Count:12
Flexural Yield Strength 62.1 - 370 MPa9000 - 53700 psiAverage value: 182 MPa Grade Count:66
 90.0 - 130 MPa
@Temperature 80.0 - 80.0 °C
13100 - 18900 psi
@Temperature 176 - 176 °F
Average value: 121 MPa Grade Count:9
Flexural Modulus 0.128 - 17.5 GPa18.6 - 2540 ksiAverage value: 9.58 GPa Grade Count:79
 6.00 - 9.00 GPa
@Temperature 80.0 - 80.0 °C
870 - 1310 ksi
@Temperature 176 - 176 °F
Average value: 7.78 GPa Grade Count:9
Izod Impact, Notched 0.534 - 3.50 J/cm1.00 - 6.56 ft-lb/inAverage value: 1.95 J/cm Grade Count:36
 0.600 - 1.30 J/cm
@Temperature -20.0 - 0.000 °C
1.12 - 2.44 ft-lb/in
@Temperature -4.00 - 32.0 °F
Average value: 0.925 J/cm Grade Count:3
Izod Impact, Unnotched 1.60 - 9.61 J/cm3.00 - 18.0 ft-lb/inAverage value: 6.74 J/cm Grade Count:12
Izod Impact, Notched (ISO) 7.00 - 29.0 kJ/m²3.33 - 13.8 ft-lb/in²Average value: 16.7 kJ/m² Grade Count:11
 15.0 - 27.0 kJ/m²
@Temperature -40.0 - -30.0 °C
7.14 - 12.8 ft-lb/in²
@Temperature -40.0 - -22.0 °F
Average value: 21.0 kJ/m² Grade Count:2
Charpy Impact Unnotched 2.00 - 8.00 J/cm²9.52 - 38.1 ft-lb/in²Average value: 5.73 J/cm² Grade Count:31
 1.80 - 8.20 J/cm²
@Temperature -40.0 - -20.0 °C
8.57 - 39.0 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 5.58 J/cm² Grade Count:20
Charpy Impact, Notched 0.500 - 5.00 J/cm²2.38 - 23.8 ft-lb/in²Average value: 2.19 J/cm² Grade Count:42
 0.400 - 4.50 J/cm²
@Temperature -40.0 - -20.0 °C
1.90 - 21.4 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 2.49 J/cm² Grade Count:22
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+15 - 2.00e+16 ohm-cm1.00e+15 - 2.00e+16 ohm-cmAverage value: 7.33e+15 ohm-cm Grade Count:6
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 - 28.8 µm/m-°C6.67 - 16.0 µin/in-°FAverage value: 19.4 µm/m-°C Grade Count:5
Melting Point 160 - 170 °C320 - 338 °FAverage value: 164 °C Grade Count:33
Maximum Service Temperature, Air 90.0 - 140 °C194 - 284 °FAverage value: 116 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 149 - 163 °C300 - 325 °FAverage value: 159 °C Grade Count:18
Deflection Temperature at 1.8 MPa (264 psi) 121 - 165 °C250 - 329 °FAverage value: 153 °C Grade Count:68
Deflection Temperature at 8.0 MPa 130 - 138 °C266 - 280 °FAverage value: 135 °C Grade Count:12
Vicat Softening Point 114 - 163 °C237 - 325 °FAverage value: 147 °C Grade Count:16
Flammability, UL94 HBHBGrade Count:27
 
Processing PropertiesMetricEnglishComments
Processing Temperature 30.0 - 290 °C86.0 - 554 °FAverage value: 152 °C Grade Count:30
Nozzle Temperature 200 - 270 °C392 - 518 °FAverage value: 236 °C Grade Count:13
Die Temperature 225 - 290 °C437 - 554 °FAverage value: 265 °C Grade Count:18
Melt Temperature 180 - 290 °C356 - 554 °FAverage value: 245 °C Grade Count:43
Mold Temperature 20.0 - 90.0 °C68.0 - 194 °FAverage value: 56.8 °C Grade Count:40
Injection Velocity 50.0 - 80.0 mm/sec1.97 - 3.15 in/secAverage value: 64.5 mm/sec Grade Count:3
Drying Temperature 70.0 - 120 °C158 - 248 °FAverage value: 88.2 °C Grade Count:40
Moisture Content 0.100 - 0.200 %0.100 - 0.200 %Average value: 0.190 % Grade Count:21
Injection Pressure 40.0 - 120 MPa5800 - 17400 psiAverage value: 87.8 MPa Grade Count:25
Hot-Working Temperature 260 - 290 °C500 - 554 °FAverage value: 275 °C Grade Count:4

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene with 40% Glass Fiber Filler
Overview of materials for Polypropylene with 30% Glass Fiber Filler
Overview of materials for Polypropylene with 10% Glass Fiber Filler
Overview of materials for Polypropylene with 60% Glass Fiber Filler
Overview of materials for Polypropylene with 20% Glass Fiber Filler

O4715 / 78380

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.