MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Overview of materials for Polypropylene with 40% Glass Fiber Filler
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 40% Glass Fiber Filler

Material Notes: This property data is a summary of similar materials in the MatWeb database for the category "Polypropylene with 40% Glass Fiber Filler". Specific grades with glass content between 35% and 44% are included. Each property range of values reported is minimum and maximum values of appropriate MatWeb entries. The comments report the average value, and number of data points used to calculate the average. The values are not necessarily typical of any specific grade, especially less common values and those that can be most affected by additives or processing methods.

Vendors: Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesMetricEnglishComments
Density 1.09 - 1.56 g/cc0.0394 - 0.0564 lb/in³Average value: 1.22 g/cc Grade Count:251
Filler Content 35.0 - 50.0 %35.0 - 50.0 %Average value: 39.7 % Grade Count:72
Water Absorption 0.000 - 0.100 %0.000 - 0.100 %Average value: 0.0383 % Grade Count:29
Additive Loading 40.0 %40.0 %Average value: 40.0 % Grade Count:5
Maximum Moisture Content 0.0100 - 0.2000.0100 - 0.200Average value: 0.162 Grade Count:5
Linear Mold Shrinkage 0.000300 - 0.0350 cm/cm0.000300 - 0.0350 in/inAverage value: 0.00320 cm/cm Grade Count:153
 0.00400 - 0.00400 cm/cm
@Temperature 80.0 - 80.0 °C
0.00400 - 0.00400 in/in
@Temperature 176 - 176 °F
Average value: 0.00222 cm/cm Grade Count:1
 0.00200 - 0.00200 cm/cm
@Temperature 220 - 240 °C
0.00200 - 0.00200 in/in
@Temperature 428 - 464 °F
Average value: 0.00222 cm/cm Grade Count:4
 0.00200 - 0.00200 cm/cm
@Pressure 60.0 - 60.0 MPa
0.00200 - 0.00200 in/in
@Pressure 8700 - 8700 psi
Average value: 0.00222 cm/cm Grade Count:4
Linear Mold Shrinkage, Transverse 0.00100 - 0.0165 cm/cm0.00100 - 0.0165 in/inAverage value: 0.00709 cm/cm Grade Count:25
 0.00800 - 0.00800 cm/cm
@Temperature 80.0 - 80.0 °C
0.00800 - 0.00800 in/in
@Temperature 176 - 176 °F
Average value: 0.00800 cm/cm Grade Count:1
Melt Flow 1.00 - 25.0 g/10 min1.00 - 25.0 g/10 minAverage value: 6.14 g/10 min Grade Count:149
Spiral Flow 20.0 - 80.0 cm7.87 - 31.5 inAverage value: 45.5 cm Grade Count:4
 106 - 106 cm
@Temperature 250 - 250 °C
41.7 - 41.7 in
@Temperature 482 - 482 °F
Average value: 106 cm Grade Count:1
 106 - 106 cm
@Thickness 2.00 - 2.00 mm
41.7 - 41.7 in
@Thickness 0.0787 - 0.0787 in
Average value: 106 cm Grade Count:1
Ash 28.0 - 40.0 %28.0 - 40.0 %Average value: 39.2 % Grade Count:11
 40.0 - 40.0 %
@Temperature 700 - 700 °C
40.0 - 40.0 %
@Temperature 1290 - 1290 °F
Average value: 40.0 % Grade Count:1
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell M 58.0 - 72.058.0 - 72.0Average value: 62.5 Grade Count:4
Hardness, Rockwell R 82.0 - 12882.0 - 128Average value: 105 Grade Count:38
Hardness, Shore D 73.0 - 85.073.0 - 85.0Average value: 76.1 Grade Count:22
Tensile Strength, Ultimate 23.4 - 170 MPa3400 - 24700 psiAverage value: 99.3 MPa Grade Count:177
 60.0 - 175.816 MPa
@Temperature -40.0 - 93.3 °C
8700 - 25500.0 psi
@Temperature -40.0 - 200 °F
Average value: 80.8 MPa Grade Count:16
Tensile Strength, Yield 3.00 - 125 MPa435 - 18100 psiAverage value: 89.7 MPa Grade Count:90
 48.0 - 48.0 MPa
@Temperature 100 - 100 °C
6960 - 6960 psi
@Temperature 212 - 212 °F
Average value: 48.0 MPa Grade Count:1
Elongation at Break 1.00 - 40.0 %1.00 - 40.0 %Average value: 3.39 % Grade Count:169
 1.80 - 5.50 %
@Temperature 4.44 - 100 °C
1.80 - 5.50 %
@Temperature 40.0 - 212 °F
Average value: 2.48 % Grade Count:17
Elongation at Yield 1.00 - 6.70 %1.00 - 6.70 %Average value: 3.24 % Grade Count:46
Modulus of Elasticity 3.59 - 12.4 GPa520 - 1800 ksiAverage value: 8.33 GPa Grade Count:127
 4.50 - 11.6521 GPa
@Temperature -40.0 - 100 °C
653 - 1690.03 ksi
@Temperature -40.0 - 212 °F
Average value: 6.55 GPa Grade Count:17
Flexural Yield Strength 50.0 - 245 MPa7250 - 35500 psiAverage value: 145 MPa Grade Count:184
 84.8055 - 293.717 MPa
@Temperature -40.0 - 93.3 °C
12300.0 - 42600.1 psi
@Temperature -40.0 - 200 °F
Average value: 124 MPa Grade Count:17
Flexural Modulus 0.120 - 12.8 GPa17.4 - 1860 ksiAverage value: 7.18 GPa Grade Count:244
 4.44022 - 11.3763 GPa
@Temperature -40.0 - 121 °C
644.010 - 1650.03 ksi
@Temperature -40.0 - 250 °F
Average value: 6.36 GPa Grade Count:16
Compressive Yield Strength 61.4 - 86.2 MPa8900 - 12500 psiAverage value: 69.6 MPa Grade Count:3
Izod Impact, Notched 0.427 - 7.52 J/cm0.800 - 14.1 ft-lb/inAverage value: 1.38 J/cm Grade Count:141
 0.500 - 3.84408 J/cm
@Temperature -40.0 - 93.3 °C
0.937 - 7.20154 ft-lb/in
@Temperature -40.0 - 200 °F
Average value: 1.53 J/cm Grade Count:7
Izod Impact, Unnotched 1.49 - 9.08 J/cm2.79 - 17.0 ft-lb/inAverage value: 5.89 J/cm Grade Count:46
 3.70 - 3.70 J/cm
@Temperature -40.0 - -40.0 °C
6.93 - 6.93 ft-lb/in
@Temperature -40.0 - -40.0 °F
Average value: 3.70 J/cm Grade Count:2
Izod Impact, Notched (ISO) 6.50 - 26.0 kJ/m²3.09 - 12.4 ft-lb/in²Average value: 13.6 kJ/m² Grade Count:22
 10.0 - 25.0 kJ/m²
@Temperature -40.0 - -20.0 °C
4.76 - 11.9 ft-lb/in²
@Temperature -40.0 - -4.00 °F
Average value: 18.3 kJ/m² Grade Count:4
Charpy Impact Unnotched 1.50 - 8.00 J/cm²7.14 - 38.1 ft-lb/in²Average value: 5.29 J/cm² Grade Count:78
 2.50 - 8.20 J/cm²
@Temperature -40.0 - 0.000 °C
11.9 - 39.0 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 5.28 J/cm² Grade Count:42
Charpy Impact, Notched 0.300 - 9.00 J/cm²1.43 - 42.8 ft-lb/in²Average value: 1.91 J/cm² Grade Count:102
 0.400 - 4.00 J/cm²
@Temperature -40.0 - 0.000 °C
1.90 - 19.0 ft-lb/in²
@Temperature -40.0 - 32.0 °F
Average value: 1.97 J/cm² Grade Count:55
Gardner Impact 0.113 - 2.26 J0.0830 - 1.67 ft-lbAverage value: 0.596 J Grade Count:28
Dart Drop, Total Energy 6.34 - 15.5 J4.68 - 11.4 ft-lbAverage value: 12.6 J Grade Count:3
 5.76 - 13.7 J
@Temperature -20.0 - -20.0 °C
4.25 - 10.1 ft-lb
@Temperature -4.00 - -4.00 °F
Average value: 9.73 J Grade Count:1
 5.76 - 13.7 J
@Thickness 3.18 - 3.18 mm
4.25 - 10.1 ft-lb
@Thickness 0.125 - 0.125 in
Average value: 9.73 J Grade Count:1
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+13 - 3.00e+16 ohm-cm1.00e+13 - 3.00e+16 ohm-cmAverage value: 7.29e+15 ohm-cm Grade Count:18
Surface Resistance 1.00e+13 - 1.00e+15 ohm1.00e+13 - 1.00e+15 ohmAverage value: 6.57e+14 ohm Grade Count:4
Dielectric Constant 2.50 - 3.202.50 - 3.20Average value: 2.94 Grade Count:6
Dielectric Strength 19.7 - 27.0 kV/mm500 - 686 kV/inAverage value: 21.6 kV/mm Grade Count:12
Dissipation Factor 0.00100 - 0.002000.00100 - 0.00200Average value: 0.00140 Grade Count:5
Arc Resistance 102 - 122 sec102 - 122 secAverage value: 109 sec Grade Count:3
Comparative Tracking Index 575 - 650 V575 - 650 VAverage value: 605 V Grade Count:5
 
Thermal PropertiesMetricEnglishComments
CTE, linear 7.92 - 60.0 µm/m-°C4.40 - 33.3 µin/in-°FAverage value: 30.7 µm/m-°C Grade Count:23
CTE, linear, Transverse to Flow 34.0 - 70.2 µm/m-°C18.9 - 39.0 µin/in-°FAverage value: 46.1 µm/m-°C Grade Count:3
Thermal Conductivity 0.346 - 0.360 W/m-K2.40 - 2.50 BTU-in/hr-ft²-°FAverage value: 0.355 W/m-K Grade Count:3
Melting Point 160 - 182 °C320 - 360 °FAverage value: 165 °C Grade Count:57
Maximum Service Temperature, Air 65.0 - 140 °C149 - 284 °FAverage value: 113 °C Grade Count:3
Deflection Temperature at 0.46 MPa (66 psi) 110 - 169 °C230 - 336 °FAverage value: 158 °C Grade Count:116
Deflection Temperature at 1.8 MPa (264 psi) 65.0 - 175 °C149 - 347 °FAverage value: 150 °C Grade Count:194
Deflection Temperature at 8.0 MPa 124 - 138 °C255 - 280 °FAverage value: 132 °C Grade Count:19
Vicat Softening Point 90.0 - 189 °C194 - 372 °FAverage value: 142 °C Grade Count:49
UL RTI, Electrical 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
UL RTI, Mechanical with Impact 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
UL RTI, Mechanical without Impact 65.0 °C149 °FAverage value: 65.0 °C Grade Count:5
Flammability, UL94 HB - V-0HB - V-0Grade Count:85
Flame Spread 22.0 - 22.9 mm/min0.866 - 0.900 in/minAverage value: 22.2 mm/min Grade Count:4
Oxygen Index 20.0 - 21.0 %20.0 - 21.0 %Average value: 20.5 % Grade Count:4
Glow Wire Test 550 - 960 °C1020 - 1760 °FAverage value: 735 °C Grade Count:11
 
Processing PropertiesMetricEnglishComments
Processing Temperature 30.0 - 290 °C86.0 - 554 °FAverage value: 176 °C Grade Count:48
Nozzle Temperature 200 - 260 °C392 - 500 °FAverage value: 234 °C Grade Count:42
Die Temperature 210 - 290 °C410 - 554 °FAverage value: 259 °C Grade Count:22
Melt Temperature 180 - 290 °C356 - 554 °FAverage value: 236 °C Grade Count:121
Mold Temperature 15.0 - 100 °C59.0 - 212 °FAverage value: 54.6 °C Grade Count:129
Injection Velocity 13.0 - 200 mm/sec0.512 - 7.87 in/secAverage value: 63.6 mm/sec Grade Count:9
Drying Temperature 60.0 - 220 °C140 - 428 °FAverage value: 89.0 °C Grade Count:111
Moisture Content 0.0200 - 0.200 %0.0200 - 0.200 %Average value: 0.127 % Grade Count:50
Injection Pressure 2.76 - 130 MPa400 - 18900 psiAverage value: 71.3 MPa Grade Count:73
Hot-Working Temperature 260 - 290 °C500 - 554 °FAverage value: 275 °C Grade Count:3

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Overview of materials for Polypropylene with 30% Glass Fiber Filler
Overview of materials for Polypropylene with 10% Glass Fiber Filler
Overview of materials for Polypropylene with 20% Glass Fiber Filler
Overview of materials for Polypropylene, Molded
Overview of materials for Polypropylene with 60% Glass Fiber Filler

O4714 / 78379

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.