Silicon Carbide, Alpha SiC
Categories: Ceramic; Carbide

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 3.10 g/cc0.112 lb/in³sintered
 3.21 g/cc0.116 lb/in³crystalline
a Lattice Constant 3.0817 Å3.0817 Å
c Lattice Constant 15.1183 Å15.1183 Å
 
Mechanical PropertiesMetricEnglishComments
Modulus of Elasticity 410 GPa59500 ksisintered
Compressive Strength 4600 MPa667000 psisintered
Poissons Ratio 0.140.14sintered
Fracture Toughness 4.60 MPa-m½4.19 ksi-in½sintered
Shear Modulus 180 GPa26100 ksiCalculated
 
Electrical PropertiesMetricEnglishComments
Magnetic Susceptibility -0.00000640-0.00000640Atomic (cgs)
Dielectric Constant 10.210.2
Band Gap 2.86 eV2.86 eV
Electron Mobility, cm²/V-s 400400
 
Thermal PropertiesMetricEnglishComments
Specific Heat Capacity 0.670 J/g-°C0.160 BTU/lb-°Fsintered
Thermal Conductivity  77.5 W/m-K
@Temperature 400 °C
538 BTU-in/hr-ft²-°F
@Temperature 752 °F
sintered
 125.6 W/m-K
@Temperature 200 °C
871.7 BTU-in/hr-ft²-°F
@Temperature 392 °F
sintered
Melting Point 2797 °C5067 °F
 
Optical PropertiesMetricEnglishComments
Refractive Index 2.672.67
 
Descriptive Properties
CAS Number409-21-2

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.