MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Copper Alloy, UNS C40950, H06 Temper, Strip
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Extra Hard

Fabrication Properties: Excellent Suitability – Soldering, Brazing, Capacity for Being Cold Worked, Capacity for Being Hot Formed; Good Suitability –Gas Shielded Arc Welding, Butt Weld; Fair Suitability – Oxyacetylene Welding, Coated Metal Arc Welding, Spot Weld, Seam Weld

Typical Uses: Connectors, automotive; Electric & Electronic parts

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.86 g/cc0.320 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Vickers 180
@Load 3.00 kg
180
@Load 6.62 lb
Tensile Strength 579 MPa84000 psiTypical
 538 - 627 MPa78000 - 91000 psi
Tensile Strength, Yield 558 MPa81000 psi0.2% Offset, Typical
 517 - 621 MPa75000 - 90000 psi0.2% Offset
Elongation at Break 3.0 %3.0 %
Tensile Modulus 120 GPa17400 ksi
Modulus of Rigidity 44.8 GPa6500 ksi
Poissons Ratio 0.340.34Calculated
Machinability 30 %30 %
Forgeability 60 %60 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000610 ohm-cm0.00000610 ohm-cm28% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear  18.0 µm/m-°C
@Temperature 20.0 - 100 °C
10.0 µin/in-°F
@Temperature 68.0 - 212 °F
 18.0 µm/m-°C
@Temperature 20.0 - 200 °C
10.0 µin/in-°F
@Temperature 68.0 - 392 °F
 18.0 µm/m-°C
@Temperature 20.0 - 300 °C
10.0 µin/in-°F
@Temperature 68.0 - 572 °F
Thermal Conductivity 14.1 W/m-K98.0 BTU-in/hr-ft²-°F
Melting Point 1040 - 1060 °C1904 - 1940 °F
Solidus 1040 °C1904 °F
Liquidus 1060 °C1940 °F
Annealing Point >= 499 °C>= 930 °F
 
Processing PropertiesMetricEnglishComments
Processing Temperature 299 °C570 °FStress Relief
Hot-Working Temperature >= 849 °C>= 1560 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 91.5 - 94.5 %91.5 - 94.5 %
Iron, Fe <= 0.030 %<= 0.030 %
Lead, Pb <= 0.050 %<= 0.050 %
Nickel, Ni 0.30 - 0.80 %0.30 - 0.80 %
Phosphorus, P 0.010 - 0.080 %0.010 - 0.080 %
Tin, Sn 0.30 - 0.80 %0.30 - 0.80 %
Zinc, Zn 3.8 - 7.9 %3.8 - 7.9 %As Balance
 
Descriptive Properties
US EPA Registered AntimicrobialYes

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC40950x2 / 291901

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.