MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Pier One Polymers PURPRENE A88 BK10 PP/EPDM Based Vulcanized TPR
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Product Description: PURPRENE A88 BK10 is a heat stabilized PP/EPDM based Thermoplastic Vulcanized Elastomer (TPV). This black compound is intended primarily for under the hood and interior applications and can be processed using Injection Molding, Extrusion, Blow Molding or other melt processing techniques. Product is supplied as free flowing pellets in 1000 Lb.

Information provided by Pier One Polymers Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 0.940 - 1.00 g/cc0.940 - 1.00 g/ccASTM D792
Melt Flow 5.0 g/10 min
@Temperature 230 °C
5.0 g/10 min
@Temperature 446 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  83 - 93
@Temperature 150 °C,
Time 605000 sec
83 - 93
@Temperature 302 °F,
Time 168 hour
Oven Air Aging; ASTM D412-98a
 83 - 93
@Temperature 135 °C,
Time 3.60e+6 sec
83 - 93
@Temperature 275 °F,
Time 1000 hour
Oven Air Aging; ASTM D412-98a
 84 - 92
@Time 5.00 sec
84 - 92
@Time 0.00139 hour
ASTM D 2240
Tensile Strength >= 9.00 MPa>= 1310 psiFlow; ASTM D412-98a
 >= 13.1 MPa>= 1900 psiPerpendicular; ASTM D412-98a
 <= 8.515 MPa
@Temperature 125 °C,
Time 252000 sec
<= 1235 psi
@Temperature 257 °F,
Time 70.0 hour
Perpendicular, Fluid Aging, IRM 903; ISO 1817
 8.515 - 14.41 MPa
@Temperature 135 °C,
Time 3.60e+6 sec
1235 - 2090 psi
@Temperature 275 °F,
Time 1000 hour
Perpendicular, Oven Air Aging; ASTM D412-98a
 9.825 - 14.41 MPa
@Temperature 150 °C,
Time 605000 sec
1425 - 2090 psi
@Temperature 302 °F,
Time 168 hour
Perpendicular, Oven Air Aging; ASTM D412-98a
Tensile Stress 5.04 - 6.16 MPa731 - 893 psi100%, Perpendicular, Oven Air Aging; ASTM D412-98a
 4.48 - 6.72 MPa650 - 975 psi100%, Perpendicular, Oven Air Aging; ASTM D412-98a
 <= 6.832 MPa<= 990.9 psi100%, Perpendicular, Fluid Aging, IRM 903; ISO 1817
 5.60 MPa
@Strain 100 %
812 psi
@Strain 100 %
Perpendicular; ASTM D412-98a
 6.00 MPa
@Strain 100 %
870 psi
@Strain 100 %
Flow; ASTM D412-98a
Elongation at Break  <= 220.5 %
@Temperature 125 °C,
Time 252000 sec
<= 220.5 %
@Temperature 257 °F,
Time 70.0 hour
Perpendicular, Fluid Aging, IRM 903; ISO 1817
 318.5 - 539 %
@Temperature 135 °C,
Time 3.60e+6 sec
318.5 - 539 %
@Temperature 275 °F,
Time 1000 hour
Perpendicular, Oven Air Aging; ASTM D412-98a
 367.5 - 539 %
@Temperature 150 °C,
Time 605000 sec
367.5 - 539 %
@Temperature 302 °F,
Time 168 hour
Perpendicular, Oven Air Aging; ASTM D412-98a
Elongation, Ultimate >= 350 %>= 350 %Flow; ASTM D412-98a
 >= 490 %>= 490 %Perpendicular; ASTM D412-98a
Tear Strength >= 7.89 kN/m>= 45.0 pliPerpendicular, 50mm/min; ASTM D1004
 >= 7.89 kN/m>= 45.0 pliFlow, 50mm/min; ASTM D1004
 <= 3.16 kN/m
@Temperature 125 °C,
Time 252000 sec
<= 18.0 pli
@Temperature 257 °F,
Time 70.0 hour
100%, Perpendicular, Fluid Aging, IRM 903
Compression Set <= 80 %
@Temperature 125 °C,
Time 252000 sec
<= 80 %
@Temperature 257 °F,
Time 70.0 hour
ASTM D-395 B
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature <= -52.0 °C<= -61.6 °FASTM D746
 
Descriptive Properties
Change in Volume<66%Fluid Aging, IRM 903, 70h @125°C
ColorBlack
Colorfastness to Light?E < 3.0
Fogging Number>70%SAE J 1756
Ozone Resistance0ISO 1431-1, “A” 100 pphm, 40°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PPIER152 / 278278

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.